Polyvinylidene fluoride trifluoroethylene film with nanorod array on surface and preparation thereof
By forming a nanorod array on a polyvinylidene fluoride trifluoroethylene film and performing corona polarization treatment, the problems of high preparation costs and uncontrollable process in the prior art are solved, and excellent piezoelectric properties and biocompatibility are obtained , suitable for biomedical implants.
Patent Information
- Application Number
- CN202411167419.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The preparation process of existing piezoelectric polymers is costly and uncontrollable, making it difficult to obtain a micro-nano structure with excellent piezoelectric properties.
Using the preparation method of polyvinylidene fluoride trifluoroethylene film, the nanorod array is formed by mixing polyvinylidene fluoride trifluoroethylene powder with N,N-dimethylformamide and forming a film on the substrate, and anodic aluminum template is used to form a nanorod array , and improve piezoelectric performance through corona polarization treatment.
A nanorod array with uniform surface distribution and highly ordered surfaces was obtained, which significantly improved piezoelectric performance and biocompatibility. It is suitable for biomedical implants and promotes cell growth and tissue repair.
Smart Images

Figure HDA0005008253100000011 
Figure HDA0005008253100000012 
Figure HDA0005008253100000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of biomedical materials, and in particular to a polyvinylidene fluoride trifluoroethylene film with a nanorod array on the surface and a preparation method thereof. Background Art
[0002] Piezoelectricity is an intrinsic property of biological tissues and plays an important role in many physiological phenomena. Piezoelectricity can be found in different parts of the human body, such as bones, tendons, skin, etc. Many functions of human cells and organs are also controlled by electrical signals.
[0003] Piezoelectric materials are a type of material that generates electrical signals when deformed. Piezoelectric materials have attracted much attention in the field of bio-electroactive materials because they can generate stable local electrical stimulation without the need for external implanted electrodes. Currently, different piezoelectric materials are used in different tissue repairs, especially in bone tissue repair and nerve tissue repair.
[0004] When bioelectroactive materials are implanted in the body, receptors on the cell membrane surface actively seek external signals provided by the implant surface in contact with them, and interactions between the biological environment and the material surface are inevitable. Cells in contact with the material can sense its surface features, integrate extracellular matrix (ECM) protein cues through signal transduction pathways, and ultimately guide the fate of the cell. Therefore, the interface between the biomaterial and the physiological environment, that is, the material surface, has a non-negligible influence on the interaction between cells and materials. Changes in cell behavior on materials are related to the specific surface properties of the material. Topological structure (roughness, porous structure, patterning), chemical characteristics (surface composition, chemical groups) and physical properties (hydrophilicity, surface energy, surface potential) are all believed to contribute to regulating cell behavior alone or in combination. These cues have been used to regulate almost all aspects of cell behavior, from cell adhesion and proliferation to proliferation and differentiation. The description of cell behavior regulated by material surface properties is crucial for the rational design of new biomaterials, implants and medical devices.
[0005] Polyvinylidene fluoride has good piezoelectricity, thermal stability, biocompatibility, etc., and is an excellent electroactive biomaterial. In recent years, a variety of polyvinylidene fluoride-based nanomaterials have been used to regulate cell behavior or promote tissue repair. Among various PVDF-based polymers, the copolymer of vinylidene fluoride and trifluoroethylene (P(VDF-TrFE)) has the best piezoelectric properties. Although the piezoelectric properties of the copolymer can be improved by optimizing the ratio of VDF / TrFE, its piezoelectric properties as a polymer are still lower than many inorganic piezoelectric ceramics and single crystals. In recent years, researchers have enhanced the piezoelectric effect of piezoelectric polymers by designing special micro-nano structures. Many new process technologies for preparing micro-nano structures have emerged. For example, electron beam lithography, ultraviolet lithography, focused ion beam, and self-assembly. For example, a Chinese patent application with publication number CN111694219A discloses a method for preparing a self-assembled three-dimensional micro-nano structure, including: surface pretreatment; spin coating SU8 photoresist; pre-baking; alignment and exposure; post-baking; development; secondary coating; pre-baking; secondary exposure; post-baking; secondary development; transfer and self-assembly to obtain a self-assembled three-dimensional micro-nano structure. However, the application of the above process technology is significantly limited due to high costs or uncontrollable processes. Therefore, it is of great value and significance to develop a new type of micro-nano structure, especially a micro-nano structure prepared with simple processes and low costs. Summary of the invention
[0006] In view of this, the present invention provides a polyvinylidene fluoride trifluoroethylene film having a nanorod array on the surface and its preparation. The preparation method of the present invention is simple and low in cost, and the obtained polyvinylidene fluoride trifluoroethylene film has a uniformly distributed and highly ordered nanorod array on the surface.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] The invention provides a polyvinylidene fluoride trifluoroethylene film, the surface of which presents a PVTF nanorod array that is evenly distributed and highly orderly arranged.
[0009] In some specific examples of the present invention, the length of the PVTF nanorod is 3 to 8 μm, and the diameter of the PVTF nanorod is 20 to 500 nm.
[0010] At the same time, the present invention also provides a method for preparing the polyvinylidene fluoride trifluoroethylene film, comprising the following steps:
[0011] S1, mixing polyvinylidene fluoride trifluoroethylene powder and N,N-dimethylformamide and stirring to obtain a solution, dropping the solution on a substrate, using a film applicator to evenly disperse the solution to form a film, and annealing to obtain a PVTF film;
[0012] S2, stacking the PVTF film on the anodized aluminum template, placing it on a hot plate to heat and keep it warm for a period of time, and then cooling it naturally with the hot plate; then immersing it in a sodium hydroxide solution to dissolve and remove the anodized aluminum template; then washing it with deionized water and ethanol for multiple times, and drying it to obtain an arrayed PVTF film;
[0013] S3, performing polarization treatment on the arrayed PVTF film.
[0014] In some specific examples of the present invention, in step S1, the feed ratio of polyvinylidene fluoride trifluoroethylene powder to N,N-dimethylformamide is 1 g: (6-12) ml, preferably 1 g: 6 ml.
[0015] In some specific examples of the present invention, in step S1, the substrate is a glass plate, preferably a tempered glass plate.
[0016] In some specific examples of the present invention, in step S1, the height of the applicator is set to 60-90 μm, preferably 70 μm.
[0017] In some specific examples of the present invention, in step S1, the temperature of the annealing treatment is 180-220°C, preferably 210°C.
[0018] In some specific examples of the present invention, in step S1, the annealing treatment time is 0.5 to 2 hours, preferably 1 hour.
[0019] In some specific examples of the present invention, in step S1, the film thickness of the PVTF film is 50-90 μm, preferably 55 μm.
[0020] In some specific examples of the present invention, in step S2, the heating temperature on the hot plate is 160-220°C, preferably 160°C.
[0021] In some specific examples of the present invention, in step S2, the heat preservation time on the hot plate is 5 to 20 minutes, preferably 5 minutes.
[0022] In some specific examples of the present invention, in step S2, the concentration of the NaOH solution is 0.05-5 mol / L, preferably 2 mol / L.
[0023] In some specific examples of the present invention, in step S2, the soaking time in the NaOH solution is 10 minutes to 24 hours, preferably 30 minutes.
[0024] In some specific examples of the present invention, in step S2, the drying temperature is 30-50°C, preferably 37°C.
[0025] In some specific examples of the present invention, in step S2, the pore size of the anodized aluminum template is 20 to 500 nm.
[0026] In some specific examples of the present invention, in step S3, the polarization treatment adopts a corona polarization method.
[0027] In some specific examples of the present invention, in step S3, the piezoelectric coefficient d of the target product obtained by the polarization treatment is 33 Satisfy: -20pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤20pC / N.
[0028] In some specific examples of the present invention, in step S3, the voltage of the high voltage electric field of the polarization treatment is 8-15 kV, and the polarization treatment time is 40-60 minutes.
[0029] In some specific examples of the present invention, in step S3, the voltage of the high voltage electric field of the polarization treatment is 8.20 kV, and the polarization treatment time is 40 min.
[0030] Compared with the prior art, the present invention has the following beneficial technical effects:
[0031] (1) The polyvinylidene fluoride trifluoroethylene film having a nanorod array on the surface of the present invention has a uniformly distributed and highly ordered PVTF nanorod array on the surface, has a high degree of orientation and crystallinity, and has significantly improved piezoelectric properties compared to unmodified PVTF films. It can provide electrical signal stimulation to cells or tissues and has good biocompatibility. It can be used as a biomedical implant to promote cell growth and tissue repair and regeneration.
[0032] (2) The preparation method of the present invention is simple to operate, relatively low in cost, and easy to control. By adjusting parameters such as heating temperature and holding time, the morphology of the surface nanorod array structure can be changed, thereby obtaining nanorod array structures with different distributions and lengths; further, by adjusting the polarization parameters, a polyvinylidene fluoride trifluoroethylene film with a nanorod array on the surface having different dipole orientation degrees and different surface potentials can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1A The XRD patterns are obtained by performing X-ray diffraction characterization on the PVTF film obtained in step (1) of this embodiment 1, the arrayed PVTF film obtained in step (2), and the target product obtained in this embodiment 1.
[0034] Figure 1BThis is a Fourier transform infrared spectrum obtained by performing Fourier transform infrared spectroscopy analysis on the PVTF film obtained in step (1) of this embodiment 1, the arrayed PVTF film obtained in step (2), and the target product obtained in this embodiment 1.
[0035] Figure 2A This is the contact angle test result of the PVTF film obtained in step (1) of Example 1.
[0036] Figure 2B It is the contact angle test result of the target product obtained in Example 1.
[0037] Figure 3A This is a SEM image of the surface morphology of the PVTF film obtained in step (1) of Example 1.
[0038] Figure 3B This is a SEM image of the surface morphology of the arrayed PVTF film obtained in step (2) of Example 1.
[0039] Figure 3C This is a SEM image of the cross-sectional morphology (part) of the arrayed PVTF film obtained in step (2) of Example 1.
[0040] Figure 3D This is a SEM image of the surface morphology of the target product obtained in Example 1.
[0041] Figure 4 This is a Kelvin probe microscope surface potential diagram of the PVTF film obtained in step (1) of Example 1.
[0042] Figure 5 This is the surface potential map of the arrayed PVTF film obtained in step (2) of Example 1 using a Kelvin probe microscope.
[0043] Figure 6 This is a surface potential map of the target product surface obtained in Example 1 using a Kelvin probe microscope.
[0044] Figure 7 This is a comparison chart of the cell viability of mouse bone marrow mesenchymal stem cells inoculated onto the target product obtained in Example 1 and the PVTF flat film obtained in step (1) after three days of culture, as determined by the CCK-8 method.
[0045] Figure 8 This is a SEM image of the surface morphology of the target product obtained in Example 2. DETAILED DESCRIPTION
[0046] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following embodiments are only used to illustrate the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0047] In the following examples, the reagents or instruments used without indicating the manufacturer are all conventional products available on the market. For example, the glass plate is a tempered glass plate, and the vinylidene fluoride-trifluoroethylene copolymer (i.e., polyvinylidene fluoride-trifluoroethylene Poly (VDF-TrFE), P (VDF-TrFE), abbreviated as PVTF) is produced by Piezotech, France, and the model is: FC30, wherein the molar ratio of vinylidene fluoride monomer to trifluoroethylene monomer is 7:3. The anodized aluminum template uses an AAO membrane with a pore size of 0.1um, the brand is GE Whatman, and the model is 6809-7013-Whatman aluminum oxide membrane.
[0048] The corona polarization device includes: a high-voltage DC power supply and a round-head electrode needle. The round-head electrode needle is placed 1 cm above the sample and connected to the positive and negative electrodes of the power supply with the negative plate below the sample. The voltage is gradually increased until the critical voltage is reached to perform corona discharge and maintained for a certain period of time.
[0049] Cell counting kit-8 was used to determine cell activity: frozen rat bone marrow mesenchymal stem cells (MSCs) were revived and cultured in DMEM low-glucose medium for 3 days, then digested with trypsin, resuspended, and prepared at a concentration of 1.0×10 5 0.5 mL of cell suspension was inoculated onto the surface of a sample with a size of 1 cm × 1 cm in each well of a 24-well plate, and then placed in a constant temperature and humidity incubator at 37 ° C and a carbon dioxide concentration of 5%, and fresh DMEM low-glucose medium was replaced every other day. After 3 days of culture, the sample was transferred to a new 24-well plate, and 500 μL of DMEM low-glucose medium and 50 μL of CCK-8 were added to each well under light-proof conditions, and incubated at 37 ° C for 2 hours, and finally the absorbance (OD value) at 450 nm was measured using an ELISA reader.
[0050] Example 1
[0051] (1) 1 g of PVTF powder was mixed with 6 ml of N,N-dimethylformamide (DMF) and magnetically stirred for 6 h to obtain a PVTF solution; the PVTF solution was dropped onto a glass plate and uniformly dispersed by an applicator to form a film. The applicator height was set to 70 μm, and the solution was annealed and crystallized in a muffle furnace at 210°C for 1 h to obtain a PVTF film with a film thickness of 55 μm;
[0052] (2) The PVTF film was washed with deionized water and ethanol and dried, and the anodized aluminum template was washed with deionized water and ethanol and dried; then, the PVTF film was stacked on the anodized aluminum template (i.e., the PVTF film was placed on the anodized aluminum template), placed on a hot plate and heated to 160°C, kept warm for 5 minutes, and then naturally cooled with the hot plate; then, the sample was immersed in a 2 mol / L NaOH solution for 30 minutes to dissolve and remove the anodized aluminum template; finally, it was washed with deionized water and ethanol several times to remove the residual NaOH solution, and dried at 37°C to obtain an arrayed PVTF film;
[0053] (3) The arrayed PVTF film obtained in step (2) is polarized by corona polarization, the voltage of the high-voltage electric field of the polarization treatment is 8.20 kV, and the polarization treatment time is 40 min to obtain the target product.
[0054] Performance and testing:
[0055] The PVTF film obtained in step (1) of this embodiment 1, the arrayed PVTF film obtained in step (2), and the target product obtained in this embodiment 1 were characterized by X-ray diffraction. The XRD patterns are as follows: Figure 1A shown. Figure 1A In the figure, the diffraction peaks at 20.7° and 38.0° correspond to the (200) and (001) reflections of the PVTFβ phase. Figure 1A It can be seen that the PVTF film, arrayed PVTF film, and target product are all β-phase PVTF crystals.
[0056] The PVTF film obtained in step (1) of this embodiment 1, the arrayed PVTF film obtained in step (2), and the target product obtained in this embodiment 1 were subjected to Fourier transform infrared spectroscopy comparative analysis, and the FTIR graphs thereof are as follows: Figure 1B shown. Figure 1B In 870cm -1 and 1279cm -1 The characteristic β phase band of PVTF is shown at Figure 1B It can be seen that the PVTF film, arrayed PVTF film, and target product are all β-phase PVTF.
[0057] The contact angles of the PVTF film obtained in step (1) and the target product obtained in step (3) of this embodiment 1 were tested respectively. The results are as follows: Figure 2A and Figure 2B As shown, the contact angles are 74.8° and 126.3°, respectively, which indicates that the hydrophilicity and hydrophobicity of the target product are greatly changed compared with that of the unmodified pure PVTF film.
[0058] The surface morphology of the PVTF film obtained in step (1) of this embodiment 1, the surface morphology of the arrayed PVTF film obtained in step (2), the cross-sectional morphology (cross-sectional section close to the surface) of the arrayed PVTF film obtained in step (2), and the surface morphology of the target product obtained in this embodiment 1 were observed using a scanning electron microscope. The SEM images are shown in FIG. Figure 3A to Figure 3D shown.
[0059] Figure 3A In the figure, the surface morphology of the PVTF film shows a typical wrinkled morphology after PVTF crystallization. Figure 3B In the figure, the surface morphology of the arrayed PVTF film appears as a highly ordered array of PVTF nanorods, with a diameter of about 200 nm. Figure 3C It can be seen that the nanorods in the cross-section close to the surface are all upright, and the morphology also presents a highly ordered array of PVTF nanorods. The length of the nanorods is about 3 μm, and the diameter of the nanorods is about 200 nm. Figure 3D In the experiment, the surface morphology of the target product is almost the same as that of the arrayed PVTF film, and it still presents a highly ordered array of PVTF nanorods, with a diameter of about 200nm. At the same time, it is also observed that the cross-sectional morphology of the target product is almost the same as that of the arrayed PVTF film, and it also presents a highly ordered array of PVTF nanorods, with a length of about 3μm and a diameter of about 200nm. It can be seen that the surface morphology of the film has changed significantly before and after the array construction: from a flat film to a highly ordered arrayed film; the surface morphology of the film remains almost unchanged before and after the polarization treatment.
[0060] The PVTF film obtained in step (1) was subjected to corona polarization and measured using a static piezoelectric coefficient D33 measuring instrument, showing that its surface piezoelectric coefficient d 33 The target product was measured using a static piezoelectric coefficient D33 measuring instrument, showing that the surface piezoelectric coefficient of the target product was d 33 It is -15pC / N. This shows that the piezoelectric performance of the target product is improved compared with the unmodified pure PVTF film.
[0061] The potential signal on the surface of the PVTF film obtained in step (1) is detected using a Kelvin probe microscope. The potential diagram is shown in FIG. Figure 4 As shown. It can be seen that the surface potential of the PVTF film is 0.09V. Using a Kelvin probe microscope, the potential signal on the surface of the arrayed PVTF film obtained in step (2) is detected, and the potential diagram is shown in Figure 5 As shown. It can be seen that the surface potential of the arrayed PVTF film is -2.45V; using a Kelvin probe microscope, the potential signal on the surface of the target product obtained in Example 1 is detected, and its potential diagram is as follows Figure 6 As shown. It can be seen that the surface potential of the target product is greater than 12 V. This result shows that after array construction, the absolute value of the surface potential of the film becomes larger; after polarization treatment, the absolute value of the surface potential of the film increases significantly.
[0062] Mouse bone marrow mesenchymal stem cells (MSCs) were inoculated onto the target product obtained in Example 1 and the PVTF flat film obtained in step (1), and the cell activity was measured using the CCK-8 method. Figure 7 As shown. Figure 7 It can be seen that the OD value of the cells inoculated with the target product obtained in Example 1 is higher than the OD value of the cells inoculated on the PVTF flat film obtained in step (1), indicating that the target product obtained in Example 1 has better cell compatibility and is more conducive to cell adhesion and proliferation.
[0063] Example 2
[0064] (1) 1 g of PVTF powder was mixed with 6 ml of N,N-dimethylformamide (DMF) and magnetically stirred for 6 h to obtain a PVTF solution; the PVTF solution was dropped onto a glass plate and uniformly dispersed by an applicator to form a film. The applicator height was set to 70 μm, and the solution was annealed and crystallized in a muffle furnace at 210°C for 1 h to obtain a PVTF film with a film thickness of 55 μm;
[0065] (2) The PVTF film was washed with deionized water and ethanol and dried, and the anodized aluminum template was washed with deionized water and ethanol and dried; then, the PVTF film was stacked on the anodized aluminum template, placed on a hot plate and heated to 190°C, kept warm for 20 minutes, and then naturally cooled with the hot plate; then, the sample was immersed in a 2 mol / L NaOH solution for 30 minutes to dissolve and remove the anodized aluminum template; finally, it was washed with deionized water and ethanol several times to remove the residual NaOH solution, and dried at 37°C to obtain an arrayed PVTF film;
[0066] (3) The arrayed PVTF film obtained in step (2) is polarized by corona polarization, the voltage of the high-voltage electric field of the polarization treatment is 8.20 kV, and the polarization treatment time is 40 min to obtain the target product.
[0067] XRD shows that the target product obtained in Example 2 is a β-phase PVTF crystal. The surface morphology of the target product obtained in Example 2 was observed using a scanning electron microscope. The SEM image is as follows: Figure 8 As shown. Figure 8 It can be seen that the surface morphology of the target product presents a highly ordered nanorod cluster structure.
[0068] The target product obtained in Example 2 was measured using a static piezoelectric coefficient D33 measuring instrument, showing that the surface piezoelectric coefficient d 33 It is -16pC / N.
[0069] Example 3
[0070] (1) 1 g of PVTF powder was mixed with 6 ml of N,N-dimethylformamide (DMF) and magnetically stirred for 6 h to obtain a PVTF solution; the PVTF solution was dropped onto a glass plate and uniformly dispersed by an applicator to form a film, the applicator height was set to 70 μm, and the solution was heat treated in a muffle furnace at 210°C for 1 h for annealing and crystallization to obtain a PVTF film with a film thickness of 55 μm;
[0071] (2) The PVTF film was washed with deionized water and ethanol and dried, and the anodized aluminum template was washed with deionized water and ethanol and dried; then, the PVTF film was stacked on the anodized aluminum template, placed on a hot plate and heated to 160°C, kept warm for 10 minutes, and then naturally cooled with the hot plate; then, the sample was immersed in a 2 mol / L NaOH solution for 30 minutes to dissolve and remove the anodized aluminum template; finally, it was washed with deionized water and ethanol several times to remove the residual NaOH solution, and dried at 37°C to obtain an arrayed PVTF film;
[0072] (3) The arrayed PVTF film obtained in step (2) is polarized by corona polarization, the voltage of the high-voltage electric field of the polarization treatment is 12.0 kV, and the polarization treatment time is 40 min to obtain the target product.
[0073] The target product obtained in Example 3 was measured using a static piezoelectric coefficient D33 measuring instrument, showing that the surface piezoelectric coefficient d of the target product obtained in Example 3 is 33 It is -18pC / N.
[0074] Based on Examples 1 to 3, it can be found that: by adjusting parameters such as heating temperature and holding time, the morphology of the surface nanorod array structure can be changed, thereby obtaining nanorod array structures of different distributions and lengths; further, by adjusting the polarization parameters, a polyvinylidene fluoride trifluoroethylene film with a nanorod array on the surface with different degrees of dipole orientation and different surface potentials can be obtained. The polyvinylidene fluoride trifluoroethylene film with a nanorod array on the surface of the present invention has good piezoelectric properties, can provide electrical signal stimulation to cells or tissues, and has good biocompatibility, so it can be used as a biomedical implant to promote cell growth and tissue repair and regeneration. In addition, the preparation method of the present invention is simple to operate and has low cost.
[0075] It can be seen that the purpose of the present invention has been completely and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments. Without departing from the principles, the implementation methods can be modified arbitrarily. Therefore, the present invention includes all modified implementation methods based on the spirit and scope of the claims.
Claims
1. A polyvinylidene fluoride trifluoroethylene film, It is characterized in that Its surface presents a uniformly distributed and highly ordered array of PVTF nanorods.
2. The polyvinylidene fluoride trifluoroethylene film according to claim 1, It is characterized in that The length of the PVTF nanorod is 3-8 μm, and the diameter of the PVTF nanorod is 20-500 nm.
3. The method for preparing the polyvinylidene fluoride trifluoroethylene film according to claim 1 or 2, It is characterized in that The following steps are involved: S1, mixing polyvinylidene fluoride trifluoroethylene powder and N,N-dimethylformamide and stirring to obtain a solution, dropping the solution on a substrate, using a film applicator to evenly disperse the solution to form a film, and annealing to obtain a PVTF film; S2, stacking the PVTF film on an anodized aluminum template, placing it on a hot plate, heating it together and keeping it warm for a period of time, and then cooling it naturally with the hot plate; Then, it was immersed in a sodium hydroxide solution to dissolve and remove the anodized aluminum template; After washing with deionized water and ethanol for several times, and drying, an arrayed PVTF film is obtained; S3, performing polarization treatment on the arrayed PVTF film.
4. The preparation method according to claim 3, It is characterized in that In the step S1, the feed ratio of polyvinylidene fluoride trifluoroethylene powder to N,N-dimethylformamide is 1 g: (6-12) ml.
5. The preparation method according to claim 3, It is characterized in that In the step S1, the film thickness of the PVTF film is 50-90 μm.
6. The preparation method according to claim 3, It is characterized in that In the step S1, the temperature of the annealing treatment is 180-220°C.
7. The preparation method according to claim 3, It is characterized in that In the step S2, the heating temperature on the hot plate is 160-220°C.
8. The preparation method according to claim 3, It is characterized in that In the step S2, the pore size of the anodized aluminum template is 20 to 500 nm.
9. The preparation method according to claim 3, It is characterized in that In the step S3, the polarization treatment adopts the corona polarization method.
10. The preparation method according to claim 9, It is characterized in that In the step S3, the voltage of the high voltage electric field of the polarization treatment is 8-15 kV, and the polarization treatment time is 40-60 minutes.
Citation Information
Patent Citations
Preparation method of self-assembled three-dimensional micro-nano structure
CN111694219A
Method for manufacturing polyvinylidene fluoride nano array pore membranes
CN104959045A
Simple preparation method for nanometer rod or nanometer wire of piezoelectric polymer
CN105576118A
Preparation method for polyvinylidene fluoride thin film electret
CN105788863A
Preparation method of polyvinylidene fluoride-based ferroelectric film with micro-nano array structure, and product and application of polyvinylidene fluoride-based ferroelectric film
CN115850779A