Aging-resistant high-weather-resistance fishing net material and preparation method thereof

By modifying the combination of polyethylene, nylon and other materials and adding composite additives, the aging problem of fishing net materials under sunlight and ultraviolet light is solved, extending the service life and improving stability, making it suitable for fishing net applications in complex environments.

CN119039681AInactive Publication Date: 2024-11-29ANHUI YISHUN FISHING NET FISHING GEAR CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411133452.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fishing net materials are prone to aging under the influence of environmental factors such as sunlight, oxygen and ultraviolet rays, resulting in short service life and reduced intensity, affecting fishing efficiency and economic benefits, and frequent replacement increases production costs and environmental pollution.

Method used

Using a combination of modified polyethylene, nylon, polyisoprene rubber, PE resin and composite additives, the antioxidant and ultraviolet absorbers of the material are enhanced by adding composite antioxidant and modified ultraviolet absorbers, and the antioxidant and ultraviolet stability of the material is enhanced, and the Lubricants and plasticizers are added to the processing to improve the physical and chemical stability of the material.

Benefits of technology

It extends the service life of the material, improves the stability and durability in harsh climates, maintains physical properties and color stability, is suitable for long-term outdoor use, and reduces the aging and degradation speed of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039681A_ABST
    Figure CN119039681A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-aging high-weather-resistance fishing net material and a preparation method thereof, and relates to the technical field of fishing nets.According to the anti-aging high-weather-resistance fishing net material, a composite antioxidant and a modified ultraviolet absorbent effectively prevent the influence of oxidation and ultraviolet radiation on the material, and the service life of the material is prolonged; the stability and durability of the material under various atrocious weather conditions are improved, the combination of modified polyethylene, nylon and simethicone enables the material to have good physical and chemical stability and not prone to deformation or degeneration, the added polyisoprene rubber enhances the flexibility and tensile property of the material, and the material has good weather resistance. The lubricant and the plasticizer are used, so that the friction and the viscosity of the material in the processing process are reduced, the extrusion molding efficiency and the quality of a finished product are improved, the long-term exposure of an outdoor environment is considered in the material design, the stability of the color and the structure is kept, and the material is suitable for being used outdoors for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fishing nets, in particular to an aging-resistant and highly weather-resistant fishing net material and a preparation method thereof. Background Art

[0002] Fishing nets are used to catch fish. In ancient times, people used coarse cloth and hemp as raw materials, and made them by bundling and rolling. Although this kind of fishing net is easy to rot and has poor toughness, its fishing efficiency has been greatly improved. With the development of the fishery, the objects of fishing and hunting are not only fish, and the tools for fishing have also kept pace with the times. In ancient times, people used coarse cloth and hemp as raw materials, and made them by bundling and rolling. Although this kind of fishing net is easy to rot and has poor toughness, its fishing efficiency has been greatly improved. With the development of the fishery, the objects of fishing and hunting are not only fish, and the tools for fishing have also kept pace with the times.

[0003] Modern fishing nets are mainly made of polyethylene, nylon and other raw materials, which have a long service life and higher fishing efficiency. However, the mechanical properties of polyethylene itself are average, with low tensile strength and poor creep resistance, which makes the strength, wear resistance and toughness of traditional fishing nets unsuitable for fishing operations in complex seabeds and windy and wave environments. They are very easy to age, which reduces the service life of fishing gear, not only wasting resources, but also directly affecting the catch. Fishing nets need to be dried after fishing. Sun exposure will promote the aging of fishing nets, shorten the service life of fishing nets, and increase additional costs;

[0004] According to the prior art, a Chinese patent with publication number "CN105367866A" discloses an anti-aging fishing net, which relates to the technical field of fishing net manufacturing. The fishing net is composed of the following components in parts by weight: 105-115 parts of polyethylene, 55-65 parts of nylon, 11-15 parts of polyisoprene rubber, 3-7 parts of dimethyl silicone oil, 6-8 parts of PE resin, 4-6 parts of polyisoprene, 2-3 parts of pentachloronitrobenzene and 7-10 parts of composite additives.

[0005] The above patent can improve the anti-aging and weather resistance of fishing nets to a certain extent. However, in the production process, polyethylene is directly used to produce fishing nets. Polyethylene is not modified. Compared with traditional polyethylene fishing nets, its anti-aging ability is limited. If only unmodified polyethylene is directly used to produce fishing nets, the anti-aging ability and weather resistance of the fishing nets will be limited. Unmodified polyethylene fishing nets are prone to aging and deterioration under the influence of environmental factors such as sunlight, oxygen, and ultraviolet rays, resulting in a shorter service life. Especially under common outdoor use conditions, unmodified polyethylene fishing nets will also lose strength and durability faster;

[0006] Aging and deterioration will cause the physical properties of fishing nets to decline, such as weakened tensile strength and poor impact resistance, making the fishing nets more susceptible to damage or breakage, thereby affecting fishing efficiency and economic benefits. Frequent replacement of aging fishing nets will also increase production costs, because short-lived fishing nets need to be replaced and maintained more frequently, which will increase labor and material costs. Frequent replacement of fishing nets will not only increase economic costs, but also lead to the generation of more waste, which will have a negative impact on the environment. It is necessary to improve the existing technology. To this end, we propose an aging-resistant and weather-resistant fishing net material and a preparation method thereof to solve the above problems. Summary of the invention

[0007] The object of the present invention is to provide a fishing net material with strong aging resistance and weather resistance and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0009] The present invention provides an aging-resistant and weather-resistant fishing net material, comprising the following materials:

[0010] By weight, they are: 105-115 parts of modified polyethylene, 55-65 parts of nylon, 11-15 parts of polyisoprene rubber, 3-7 parts of dimethyl silicone oil, 6-8 parts of PE resin, 4-6 parts of polyisoprene, 2-3 parts of pentachloronitrobenzene and 7-10 parts of composite additives;

[0011] The composite auxiliary agent is composed of the following components in parts by weight: 1.6-1.8 parts of zinc borate, 1.9-2.3 parts of phenolic resin, 1.7-1.9 parts of sodium citrate, 1.4-1.7 parts of dioctyl fat, 1.2-1.5 parts of methyl ethyl ketone peroxide and 2.4-2.7 parts of nano titanium dioxide.

[0012] Preferably, the preparation method of the composite auxiliary agent is: adding sodium citrate and phenolic resin to a mixture of other ingredients, heating while stirring, stirring for 30-45 minutes, and controlling the temperature to 165°C-185°C, to obtain the composite auxiliary agent.

[0013] Preferably, the modified polyethylene comprises 70-85 parts of polyethylene, 5-12 parts of composite antioxidant, 4-10 parts of modified ultraviolet absorber, 3-6 parts of plasticizer and 0.5-1.5 parts of lubricant.

[0014] Preferably, the composite antioxidant is composed of a hindered phenol antioxidant and a thioester antioxidant, and the mass ratio of the two is (0.8-1.2):1.

[0015] Preferably, the preparation of the hindered phenol antioxidant comprises the following steps:

[0016] A101, dissolving 4,4'-methylenebis(2,6-diethylaniline) in a first organic solvent, adding dropwise an acid binding agent at 0-4°C, adding dropwise a mixed solution of the first organic solvent and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride under an inert gas protection atmosphere, heating to react, and obtaining a reaction solution;

[0017] A102, distilling the reaction solution under reduced pressure to obtain an intermediate reactant;

[0018] A103, dissolving the obtained intermediate reactant in a second organic solvent, washing with an acid solution and a saturated sodium chloride solution in sequence, and then performing reduced pressure distillation to obtain a solid reactant;

[0019] A104. Dissolve the obtained solid reactant in a third organic solvent, add an alkaline solution to precipitate the solid, and then wash the obtained solid with deionized water and dry it to obtain a hindered phenol antioxidant.

[0020] Preferably, the molar ratio of the 4,4'-methylenebis(2,6-diethylaniline) to β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride is 1:(2.2-2.8).

[0021] Preferably, the preparation of the modified ultraviolet absorber comprises the following steps:

[0022] B101, dissolving 3-(3-hydroxy-3-methylbutane)-2,4,6-trihydroxybenzophenone in a solvent, adding a catalyst under an inert gas atmosphere, heating to 65-80° C., gradually dropping 1-allyl-3-chloro-5-fluorobenzene, controlling the dropping time to 2-3 hours, and reacting at a constant temperature for 20-40 minutes after the dropping is completed to obtain a reaction product;

[0023] B102. Add ethanol to the reaction product to dissolve the remaining unreacted substances, filter to obtain a solid, wash and dry the filtered product to obtain a modified ultraviolet absorber.

[0024] Preferably, the molar ratio of the 3-(3-hydroxy-3-methylbutanyl)-2,4,6-trihydroxybenzophenone to 1-allyl-3-chloro-5-fluorobenzene is 1:(1.2-2.6).

[0025] Preferably, the specific preparation process of the modified polyethylene is:

[0026] C101 and polyethylene were added into the reaction kettle, stirred at 120-150°C for 60-80min, then cooled to 35-40°C, and stirred for 20-30min at a stirring rate of 120-150r / min to obtain a mixture A;

[0027] C102, adding a composite antioxidant, a modified ultraviolet absorber, a plasticizer, and a lubricant to the mixture A, heating to 80-120° C., pressurizing to 0.8-1.2 MPa, stirring for 40-60 min at a stirring rate of 160-200 r / min, standing and cooling to room temperature to obtain a mixture B;

[0028] C103. Filter the mixture B, introduce it into a parallel twin-screw extruder for extrusion granulation and dry it to obtain modified polyethylene.

[0029] A method for preparing an aging-resistant and weather-resistant fishing net material comprises the following specific steps:

[0030] S101, add 105-115 parts of modified polyethylene, 55-65 parts of nylon and 3-7 parts of dimethyl silicone oil into a blender and stir evenly for 11-20 minutes;

[0031] S101, placing the uniformly stirred mixture into a reactor, adding 11-15 of polyisoprene rubber, 6-8 of PE resin and 4-6 of polyisoprene, controlling the temperature to 175° C.-190° C., and reacting for 23-40 minutes;

[0032] S103, adding pentachloronitrobenzene 2-3 and composite auxiliary agent 7-10 to the reaction mixture, stirring evenly, stirring time is 18-23 minutes, and then heating to a molten state, and the heating temperature is controlled to be 130°C-155°C;

[0033] S104, adding the molten mixture into an extruder, extruding and molding, and obtaining a fishing net material.

[0034] Compared with the prior art, one or more of the above technical solutions have the following beneficial effects:

[0035] The composite antioxidant and modified ultraviolet absorber in the present invention effectively prevent the influence of oxidation and ultraviolet radiation on the material, and extend the service life of the material. The addition of the composite auxiliary agent improves the stability and durability of the material under various adverse climatic conditions. The combination of modified polyethylene, nylon and dimethyl silicone oil enables the material to have good physical and chemical stability and is not easy to deform or degrade. The added polyisoprene rubber enhances the flexibility and tensile strength of the material, making it more suitable as a fishing net material. The use of lubricants and plasticizers reduces the friction and viscosity of the material during processing, improves the efficiency of extrusion molding and the quality of the finished product. The material design takes into account the long-term exposure to the outdoor environment, maintains the stability of color and structure, and is suitable for long-term outdoor use. The improved polyethylene fishing net material not only has improved functional performance, but also can meet the needs in various complex environments. It is an advanced material with broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0037] Figure 1 It is a schematic diagram of the structure of the preparation process of the aging-resistant and weather-resistant fishing net material of the present invention;

[0038] Figure 2 It is a structural schematic diagram of the preparation process of the hindered phenol antioxidant of the present invention;

[0039] Figure 3 It is a schematic diagram of the structure of the preparation process of the modified ultraviolet absorber of the present invention;

[0040] Figure 4 It is a structural schematic diagram of the modified polyethylene preparation process of the present invention; DETAILED DESCRIPTION

[0041] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.

[0042] See also Figure 1-Figure 4 The present invention provides a fishing net material with strong aging and weather resistance, including the following materials:

[0043] The weight ratios are as follows: 105-115 parts of modified polyethylene, 55-65 parts of nylon, 11-15 parts of polyisoprene rubber, 3-7 parts of dimethyl silicone oil, 6-8 parts of PE resin, 4-6 parts of polyisoprene, 2-3 parts of pentachloronitrobenzene and 7-10 parts of composite additives; the composite additives are composed of the following components in parts by weight: 1.6-1.8 parts of zinc borate, 1.9-2.3 parts of phenolic resin, 1.7-1.9 parts of sodium citrate, 1.4-1.7 parts of dioctyl ester, 1.2-1.5 parts of methyl ethyl ketone peroxide and 2.4-2.7 parts of nano titanium dioxide; the preparation method of the composite additive is as follows: adding sodium citrate and phenolic resin to a mixture of other components, heating while stirring for 30-45 minutes, and controlling the temperature to be 165-185°C to obtain the composite additive, and these components can enhance the weather resistance and anti-aging properties of the material.

[0044] The specific material of the modified polyethylene is: 70-85 parts of polyethylene, 5-12 parts of composite antioxidant, 4-10 parts of modified ultraviolet absorber, 3-6 parts of plasticizer and 0.5-1.5 parts of lubricant.

[0045] The composite antioxidant is composed of a hindered phenol antioxidant and a thioester antioxidant, and the mass ratio of the two is (0.8-1.2):1; 4,4'-methylenebis(2,6-diethylaniline) is dissolved in a first organic solvent, an acid-binding agent is added dropwise at 0-4°C, a mixed solution of the first organic solvent and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl chloride is added dropwise under an inert gas protection atmosphere, and the mixture is heated to react to obtain a reaction solution, and the reaction solution is subjected to reduced pressure distillation to obtain The intermediate reactant is dissolved in a second organic solvent, washed with an acid solution and a saturated sodium chloride solution in sequence, and then subjected to reduced pressure distillation to obtain a solid reactant, the solid reactant is dissolved in a third organic solvent, an alkali solution is added to precipitate the solid, and the solid is washed with deionized water and then dried to obtain a hindered phenol antioxidant, 4,4'-methylenebis(2,6-diethylaniline) and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride in a molar ratio of 1:

[0046] (2.2-2.8), thereby obtaining a hindered phenol antioxidant, and through a series of chemical reactions, including synthesis reaction, solvent dissolution and washing process, finally obtaining a compound with antioxidant effect. The composite antioxidant can effectively extend the service life of the material and resist oxidation and degradation in the external environment.

[0047] 3-(3-hydroxy-3-methylbutyl)-2,4,6-trihydroxybenzophenone is dissolved in a solvent, a catalyst is added under an inert gas atmosphere, the mixture is heated to 65-80°C, 1-allyl-3-chloro-5-fluorobenzene is gradually added dropwise, the addition time is controlled to be 2-3h, and the reaction is carried out at a constant temperature for 20-40min after the addition is completed to obtain a reaction product, ethanol is added to the reaction product to dissolve the remaining unreacted substances, a solid is obtained by filtering, and the filtered product is washed and dried to obtain a modified ultraviolet absorber, wherein the molar ratio of 3-(3-hydroxy-3-methylbutyl)-2,4,6-trihydroxybenzophenone to 1-allyl-3-chloro-5-fluorobenzene is 1:

[0048] (1.2-2.6); a modified UV absorber is obtained through a synthetic reaction to ensure that the material can effectively absorb ultraviolet rays under sunlight exposure to prevent aging and discoloration of the material. The modified UV absorber improves the weather resistance of the material, allowing it to maintain the stability of color and structure when used outdoors for a long time.

[0049] The plasticizer is any one or more of dicyclohexyl phthalate, dioctyl phthalate and di(2-ethylhexyl) phthalate, and the lubricant is any one or more of erucamide, stearic acid ethylene diamide and oleic acid amide. A variety of phthalate compounds are selectively used to improve the flexibility and processability of the material. By adding erucamide, stearic acid ethylene diamide, etc., the friction and viscosity of the material during the processing process are reduced, and the efficiency and quality of extrusion molding are improved.

[0050] Finally, polyethylene is added to the reactor, stirred at 120-150°C for 60-80 minutes, then cooled to 35-40°C, and stirred for 20-30 minutes at a stirring rate of 120-150r / min to obtain a mixture A; a composite antioxidant, a modified ultraviolet absorber, a plasticizer, and a lubricant are added to the mixture A, heated to 80-120°C, pressurized at 0.8-1.2Mpa, stirred for 40-60 minutes at a stirring rate of 160-200r / min, allowed to stand and cooled to room temperature to obtain a mixture B; the mixture B is filtered, introduced into a parallel twin-screw extruder for extrusion granulation and dried to obtain a modified polyethylene, and the modified polyethylene has good aging resistance and UV resistance, which enable it to maintain stability and durability when used for a long time in outdoor environments.

[0051] Comparative Example 1

[0052] 105-115 parts of polyethylene, 55-65 parts of nylon and 3-7 parts of dimethyl silicone oil are added to a mixer and stirred evenly for 11-20 minutes. The stirred mixture is put into a reactor, and 11-15 parts of polyisoprene rubber, 6-8 parts of PE resin and 4-6 parts of polyisoprene are added. The temperature is controlled at 175°C-190°C and the reaction time is 23-40 minutes. 2-3 parts of pentachloronitrobenzene and 7-10 parts of composite additives are added to the reacted mixture, stirred evenly for 18-23 minutes, and then heated to a molten state at a heating temperature of 130°C-155°C. The molten mixture is added to an extruder and extruded to obtain a non-modified polyethylene fishing net material.

[0053] Performance test of non-modified polyethylene fishing net materials:

[0054] (1) Light aging test: Use a UV aging tester to continuously expose the manufactured PE board to a UV light source for 30 days, and observe whether there is any color change or crack on the surface;

[0055] (2) Tensile strength: Test the tensile strength of the PE board before and after irradiation with a UV aging tester;

[0056] Table 1

[0057] UV exposure / day Degree of photoaging Tensile strength / Mpa 5 No change 43.2 10 No change 43.1 15 No change 43 20 No change 42.8 25 Color changes, no cracks 38.5 30 Color changes, slight cracks 34.3 35 Color changes, slight cracks 32.5

[0058] Example 2

[0059] Add 105-115 parts of modified polyethylene, 55-65 parts of nylon and 3-7 parts of dimethyl silicone oil into a mixer and stir evenly for 11-20 minutes. Put the evenly stirred mixture into a reactor, add 11-15 parts of polyisoprene rubber, 6-8 parts of PE resin and 4-6 parts of polyisodiene, control the temperature to 175℃-190℃, and react for 23-40 minutes. Add 2-3 parts of pentachloronitrobenzene and 7-10 parts of composite additives to the reacted mixture, stir evenly for 18-23 minutes, then heat to a molten state, control the heating temperature to 130℃-155℃, add the molten state mixture into an extruder, extrude and shape, and obtain a modified polyethylene fishing net material.

[0060] Performance test of modified polyethylene fishing net material:

[0061] (1) Light aging test: Use a UV aging tester to continuously expose the manufactured PE board to a UV light source for 30 days, and observe whether there is any color change or crack on the surface;

[0062] (2) Tensile strength: Test the tensile strength of PE board before and after irradiation by UV aging tester

[0063]

[0064]

[0065] From the data in Table 1 and Table 2, we can analyze and compare the performance of polyethylene fishing net materials under two different treatment methods in more detail:

[0066] Unmodified polyethylene fishing net material:

[0067] Light aging performance:

[0068] Under ultraviolet irradiation, the material began to change color from the 25th day, and slight cracks appeared on the surface on the 30th day. This shows that the surface of the material gradually loses its original appearance characteristics under long-term ultraviolet irradiation, and structural damage may occur.

[0069] Tensile Strength:

[0070] After the light aging test, the tensile strength began to decrease significantly from the 25th day, especially after the 30th day, the decline rate accelerated. This rapid decrease in strength may affect the durability and safety of the material in use.

[0071] Modified polyethylene fishing net materials:

[0072] Light aging performance:

[0073] The material began to show changes in surface color on the 35th day, but no surface cracks were observed during the entire test period. This shows that the modification treatment can delay the appearance change and structural damage of the material under UV light.

[0074] Tensile Strength:

[0075] The decline rate of tensile strength is relatively slow, especially in the later stage of light aging test (after the 30th day). This property shows that the modification treatment effectively maintains the mechanical strength and service life of the material, and it has a longer service life and better durability than the non-modified material.

[0076] After long-term exposure to ultraviolet rays, the modified polyethylene fishing net material shows better weather resistance and tensile strength retention. This modification treatment can not only delay the surface aging and structural damage of the material, but also effectively improve the stability and service life of the material in outdoor environments. It is suitable for application scenarios with long-term exposure to ultraviolet rays and is suitable for the preparation of fishing net materials.

[0077] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A fishing net material with strong aging and weather resistance, characterized in that: The following materials are included: By weight, they are: 105-115 parts of modified polyethylene, 55-65 parts of nylon, 11-15 parts of polyisoprene rubber, 3-7 parts of dimethyl silicone oil, 6-8 parts of PE resin, 4-6 parts of polyisoprene, 2-3 parts of pentachloronitrobenzene and 7-10 parts of composite additives; The composite auxiliary agent is composed of the following components in parts by weight: 1.6-1.8 parts of zinc borate, 1.9-2.3 parts of phenolic resin, 1.7-1.9 parts of sodium citrate, 1.4-1.7 parts of dioctyl fat, 1.2-1.5 parts of methyl ethyl ketone peroxide and 2.4-2.7 parts of nano titanium dioxide.

2. The aging-resistant and weather-resistant fishing net material according to claim 1, characterized in that: The preparation method of the composite auxiliary agent is as follows: sodium citrate and phenolic resin are added to a mixture of other components, and the mixture is heated while being stirred for 30-45 minutes, and the temperature is controlled at 165° C.-185° C., so as to obtain the composite auxiliary agent.

3. The aging-resistant and weather-resistant fishing net material according to claim 1, characterized in that: The specific material of the modified polyethylene is: 70-85 parts of polyethylene, 5-12 parts of composite antioxidant, 4-10 parts of modified ultraviolet absorber, 3-6 parts of plasticizer and 0.5-1.5 parts of lubricant.

4. The aging-resistant and weather-resistant fishing net material according to claim 3, characterized in that: The composite antioxidant is composed of a hindered phenol antioxidant and a thioester antioxidant, and the mass ratio of the two is (0.8-1.2):

1.

5. The aging-resistant and weather-resistant fishing net material according to claim 4, characterized in that: The preparation of the hindered phenol antioxidant comprises the following steps: A101, dissolving 4,4'-methylenebis(2,6-diethylaniline) in a first organic solvent, adding dropwise an acid binding agent at 0-4°C, adding dropwise a mixed solution of the first organic solvent and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride under an inert gas protection atmosphere, heating to react, and obtaining a reaction solution; A102, distilling the reaction solution under reduced pressure to obtain an intermediate reactant; A103, dissolving the obtained intermediate reactant in a second organic solvent, washing with an acid solution and a saturated sodium chloride solution in sequence, and then performing reduced pressure distillation to obtain a solid reactant; A104. Dissolve the obtained solid reactant in a third organic solvent, add an alkaline solution to precipitate the solid, and then wash the obtained solid with deionized water and dry it to obtain a hindered phenol antioxidant.

6. The aging-resistant and weather-resistant fishing net material according to claim 5, characterized in that: The molar ratio of the 4,4'-methylenebis(2,6-diethylaniline) to β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride is 1:(2.2-2.8).

7. The aging-resistant and weather-resistant fishing net material according to claim 3, characterized in that: The preparation of the modified ultraviolet absorber comprises the following steps: B101, dissolving 3-(3-hydroxy-3-methylbutane)-2,4,6-trihydroxybenzophenone in a solvent, adding a catalyst under an inert gas atmosphere, heating to 65-80° C., gradually dropping 1-allyl-3-chloro-5-fluorobenzene, controlling the dropping time to 2-3 hours, and reacting at a constant temperature for 20-40 minutes after the dropping is completed to obtain a reaction product; B102. Add ethanol to the reaction product to dissolve the remaining unreacted substances, filter to obtain a solid, wash and dry the filtered product to obtain a modified ultraviolet absorber.

8. The aging-resistant and weather-resistant fishing net material according to claim 7, characterized in that: The molar ratio of the 3-(3-hydroxy-3-methylbutanyl)-2,4,6-trihydroxybenzophenone to 1-allyl-3-chloro-5-fluorobenzene is 1:(1.2-2.6).

9. The aging-resistant and weather-resistant fishing net material according to claim 3, characterized in that: The specific preparation process of the modified polyethylene is as follows: C101 and polyethylene were added into the reaction kettle, stirred at 120-150°C for 60-80min, then cooled to 35-40°C, and stirred for 20-30min at a stirring rate of 120-150r / min to obtain a mixture A; C102, adding a composite antioxidant, a modified ultraviolet absorber, a plasticizer, and a lubricant to the mixture A, heating to 80-120° C., pressurizing to 0.8-1.2 MPa, stirring for 40-60 min at a stirring rate of 160-200 r / min, standing and cooling to room temperature to obtain a mixture B; C103. Filter the mixture B, introduce it into a parallel twin-screw extruder for extrusion granulation and dry it to obtain modified polyethylene.

10. The method for preparing an aging-resistant and weather-resistant fishing net material according to claim 1, characterized in that: The specific steps include: S101, add 105-115 parts of modified polyethylene, 55-65 parts of nylon and 3-7 parts of dimethyl silicone oil into a blender and stir evenly for 11-20 minutes; S101, placing the uniformly stirred mixture into a reactor, adding 11-15 of polyisoprene rubber, 6-8 of PE resin and 4-6 of polyisoprene, controlling the temperature to 175° C.-190° C., and reacting for 23-40 minutes; S103, adding pentachloronitrobenzene 2-3 and composite auxiliary agent 7-10 to the reaction mixture, stirring evenly, stirring time is 18-23 minutes, and then heating to a molten state, and the heating temperature is controlled to be 130°C-155°C; S104, adding the molten mixture into an extruder, extruding and molding, and obtaining a fishing net material.

Citation Information

Cited By

  • High and low temperature resistant silicone rubber as well as preparation method and application thereof

    CN121851726A