Temperature-resistant wear-resistant self-lubricating gasket material and preparation method thereof
Through the composite treatment of polytetrafluoroethylene fabrics with prepreg solution A and impregnation solution B, the problem of insufficient mechanical and thermal conductivity of polytetrafluoroethylene self-lubricating pad material is solved, and high-performance temperature, wear and self-lubricating resistance is achieved The padding material is suitable for high temperature, high load and high friction environments.
Patent Information
- Application Number
- CN202411153498.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing polytetrafluoroethylene self-lubricating pad materials have poor mechanical properties, insufficient thermal conductivity and friction resistance, and poor dispersion of graphene in polytetrafluoroethylene substrates, resulting in limited overall performance improvement.
The composite material of polytetrafluoroethylene fabrics, prepreg solution A and impregnation solution B is used. The prepreg solution A contains graphene and sulfonic acid dispersant, and the impregnation solution B contains polytetrafluoroethylene ultrafine powder, engineering resin and nanofiller. The composite material is formed by sonication and multiple impregnation, scratching and extrusion, and a temperature-resistant and wear-resistant self-lubricating pad material is obtained by molding.
Improve the mechanical properties, thermal conductivity and friction resistance of self-lubricating pad materials, enhance the mechanical properties of polytetrafluoroethylene fibers, promote the dispersion of graphene, ensure the low friction performance of the material, and is suitable for high temperature and high loads. , high friction conditions.
Smart Images

Figure BDA0005004252260000051 
Figure BDA0005004252260000052 
Figure BDA0005004252260000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a heat-resistant, wear-resistant, self-lubricating liner material and a preparation method thereof. Background Art
[0002] As a self-lubricating polymer material, polytetrafluoroethylene is widely used in self-lubricating gaskets. However, polytetrafluoroethylene has poor mechanical properties, low mechanical strength and high wear rate, so it needs to be compounded with other materials to improve its comprehensive performance.
[0003] In the prior art, people often use fiber materials, nanomaterials, metal powders and other materials as fillers, and compound them with polytetrafluoroethylene substrates to form self-lubricating gasket materials to improve the mechanical and friction resistance of lubricating gasket materials. However, due to the high crystallinity and non-polarity of polytetrafluoroethylene itself, it has a very low surface energy, resulting in poor wettability of polytetrafluoroethylene substrates and poor adhesion to other materials, which leads to no obvious improvement in the mechanical and friction resistance of self-lubricating gasket materials. At the same time, in order to improve the thermal conductivity of self-lubricating gasket materials, people try to add graphene to polytetrafluoroethylene substrates, but the dispersibility of graphene in polytetrafluoroethylene substrates is poor, and with the increase of the amount of graphene added, not only does it fail to improve the overall thermal conductivity of the self-lubricating gasket material, but it also increases the friction coefficient of the self-lubricating gasket material, resulting in poor friction resistance.
[0004] In view of the problems existing in the prior art, how to develop a temperature-resistant, wear-resistant, self-lubricating liner material with good mechanical properties, friction resistance and thermal conductivity is a problem to be solved urgently in the present invention. Summary of the invention
[0005] The object of the present invention is to provide a temperature-resistant, wear-resistant, self-lubricating lining material to solve the problems raised in the above-mentioned background technology.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: On the one hand, the present invention provides a heat-resistant and wear-resistant self-lubricating gasket material, the raw materials for preparing the material include polytetrafluoroethylene fabric, pre-impregnation liquid A and impregnation liquid B, the raw materials for preparing the pre-impregnation liquid A include graphene and sulfonic acid type dispersant; the raw materials for preparing the impregnation liquid B include polytetrafluoroethylene ultrafine powder, engineering resin and nanofiller; the raw materials for preparing the sulfonic acid type dispersant include phthalic anhydride, diethylene glycol, maleic anhydride and sodium bisulfite.
[0007] As a further improvement, the preparation method of the sulfonic acid type dispersant comprises the following steps: firstly subjecting phthalic anhydride and diethylene glycol to a ring-opening esterification reaction, using p-toluenesulfonic acid as a catalyst, to obtain an intermediate 1; then subjecting the obtained intermediate 1 to a reaction with maleic anhydride under the condition of p-toluenesulfonic acid as a catalyst, to obtain an intermediate 2; adding a sodium hydroxide aqueous solution to adjust the pH of the reaction solution; and finally adding sodium bisulfite to carry out a sulfonation reaction, to obtain a sulfonic acid type dispersant.
[0008] As a further improvement, the mass ratio of the engineering resin to the nanofiller in the impregnation liquid B is 1:(0.3-1).
[0009] As a further improvement, the pre-impregnation liquid A further comprises a surfactant, and the surfactant is a secondary alcohol polyoxyethylene ether.
[0010] As a further improvement, the engineering resin includes one or more of phenolic resin, polyimide resin and epoxy resin.
[0011] As a further improvement, the nano filler comprises one or more of nano titanium dioxide, nano aluminum oxide or nano silicon dioxide.
[0012] As a further improvement, the mass ratio of graphene to sulfonic acid dispersant in the pre-impregnation liquid A is 1:(0.5-1), and the mass ratio of polytetrafluoroethylene ultrafine powder to the total mass of engineering resin and nanofiller in the impregnation liquid B is 1:(0.5-0.9).
[0013] As a further improvement, the raw materials for preparing the polytetrafluoroethylene fabric include aramid fibers and polytetrafluoroethylene fibers, the specifications of the aramid fibers are 400-1000D filaments, and the specifications of the polytetrafluoroethylene fibers are 200-600D filaments.
[0014] In another aspect, the present invention provides a method for preparing a heat-resistant, wear-resistant, self-lubricating liner material, comprising the following steps:
[0015] S1: preparing polytetrafluoroethylene fabric, weaving aramid fiber as warp yarn and polytetrafluoroethylene fiber as weft yarn to obtain polytetrafluoroethylene fabric; the weaving method is one of plain weaving method, twill weaving method or satin weaving method.
[0016] S2: preparing pre-impregnation liquid A, mixing graphene and sulfonic acid dispersant, adding them to deionized water, and ultrasonicating for 40-60 minutes to obtain pre-impregnation liquid A for standby use; preparing impregnation liquid B, mixing polytetrafluoroethylene ultrafine powder, engineering resin and nanofiller, adding them to ethanol solution, and ultrasonicating for 40-60 minutes to obtain impregnation liquid B for standby use;
[0017] S3: impregnating the polytetrafluoroethylene fabric prepared in S1 into the pre-impregnation liquid A for 60-180 minutes and then drying, and the above fabric impregnation is repeated for 5-80 times to obtain a modified polytetrafluoroethylene fabric;
[0018] S4: Soaking the modified polytetrafluoroethylene fabric in the impregnation liquid B, repeatedly scraping and squeezing for 30-40 minutes to obtain an impregnated composite material; then compression molding the impregnated composite material to obtain a heat-resistant, wear-resistant, self-lubricating liner material.
[0019] As a further improvement, the compression molding pressure conditions are 15-40 MPa, the temperature is 330-340° C., and the holding time is 1-4 h.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: the heat-resistant and wear-resistant self-lubricating gasket material provided by the present invention has good mechanical properties, thermal conductivity and friction resistance. This type of heat-resistant and wear-resistant self-lubricating gasket material reduces the introduction of other reinforcements, improves the interface bonding of the composite material, and enhances the mechanical properties of polytetrafluoroethylene fiber; the combination of sulfonic acid dispersant and secondary alcohol polyoxyethylene ether promotes the dispersion of graphene, enhances the thermal conductivity of the self-lubricating gasket material, and ensures the low friction performance of the self-lubricating gasket material, which is conducive to the application of this type of material in high temperature, high load, and high friction conditions. DETAILED DESCRIPTION
[0021] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0022] In the following examples, the compound monomers and related reagents used can be purchased from the market, among which aramid fiber was purchased from Guangdong Tewilong New Material Application Co., Ltd., polytetrafluoroethylene fiber was purchased from Nantong Kejia Textile Fiber Products Co., Ltd., polytetrafluoroethylene ultrafine powder was purchased from Shunbang New Materials Factory, Zhangqiu District, Jinan City, phenolic resin was purchased from Shenzhen Yoshida Chemical Co., Ltd. with a brand name of 2123, nano titanium dioxide was purchased from Changzhou Quantong Chemical Co., Ltd. with a brand name of R930, graphene was purchased from Shenzhen Guosen Linghang Technology Co., Ltd., and secondary alcohol polyoxyethylene ether and fatty alcohol polyoxyethylene ether were purchased from Shanghai Huijun Chemical Co., Ltd.
[0023] The following examples and comparative examples all comprise the following steps:
[0024] Preparation of sulfonic acid dispersant A: 14.8 g of phthalic anhydride, 21.2 g of diethylene glycol, and 0.172 g of p-toluenesulfonic acid are put into a flask, and the mixture is stirred and reacted at 185°C for 10 hours. 19.6 g of maleic anhydride and 0.172 g of p-toluenesulfonic acid are continuously added to the reaction solution, and the mixture is stirred and reacted at 120°C for 5 hours. Then, 1 mol / L aqueous sodium hydroxide solution is added to adjust the pH of the reaction solution to 7. Finally, 25.2 g of sodium bisulfite is added, and the mixture is stirred and reacted at 90°C for 5 hours to obtain the sulfonic acid dispersant A.
[0025] A method for preparing a heat-resistant, wear-resistant, self-lubricating liner material comprises the following steps:
[0026] S1: preparing a polytetrafluoroethylene fabric, weaving it with aramid fiber 600D filament as warp yarn and polytetrafluoroethylene fiber 400D filament as weft yarn, using a plain weave method to weave, and cutting the polytetrafluoroethylene fabric into 5 cm×5 cm sizes for standby use;
[0027] S2: Preparing pre-impregnation liquid A, according to the contents in Table 1, mixing graphene, dispersant and surfactant, and then adding them to deionized water, ultrasonicating for 60 minutes, to obtain pre-impregnation liquid A for standby use; preparing impregnation liquid B, according to the contents in Table 2, mixing polytetrafluoroethylene ultrafine powder, engineering resin and nanofiller, adding them to 95% ethanol aqueous solution, ultrasonicating for 60 minutes, to obtain impregnation liquid B for standby use;
[0028] S3: Cut the polytetrafluoroethylene fabric prepared in S1 into 5 cm×5 cm polytetrafluoroethylene fabrics and immerse them in the pre-impregnation liquid A for 180 min and then dry them. Repeat the above immersion and drying operations 20 times to obtain a modified polytetrafluoroethylene fabric;
[0029] S4: Soak 10 g of modified polytetrafluoroethylene fabric in impregnation liquid B, repeatedly stir, scrape and squeeze for 40 minutes to obtain an impregnated composite material; then the impregnated composite material is compression molded under a pressure condition of 15 MPa, a temperature of 350°C, and a holding time of 4 hours to obtain a heat-resistant, wear-resistant, self-lubricating liner material.
[0030] Table 1 Components and contents of pre-impregnation solution A
[0031]
[0032] Table 2 Composition and content of impregnation solution B
[0033]
[0034]
[0035] Example 1 provides a temperature-resistant, wear-resistant, self-lubricating gasket material, comprising the following components: polytetrafluoroethylene fabric, pre-impregnation liquid A1 and impregnation liquid B1.
[0036] Example 2 provides a temperature-resistant, wear-resistant, self-lubricating lining material, comprising the following components: polytetrafluoroethylene fabric, pre-impregnation liquid A2 and impregnation liquid B2.
[0037] Example 3 provides a temperature-resistant, wear-resistant, self-lubricating lining material, comprising the following components: polytetrafluoroethylene fabric, pre-impregnation liquid A3 and impregnation liquid B3.
[0038] Example 4 provides a temperature-resistant, wear-resistant, self-lubricating gasket material, comprising the following components: polytetrafluoroethylene fabric, pre-impregnation liquid A1 and impregnation liquid B4.
[0039] Example 5 provides a temperature-resistant, wear-resistant, self-lubricating gasket material, comprising the following components: polytetrafluoroethylene fabric, pre-impregnation liquid A1 and impregnation liquid B5.
[0040] Comparative Example 1 provides a temperature-resistant, wear-resistant, self-lubricating gasket material, comprising the following components: polytetrafluoroethylene fabric, pre-impregnation liquid A4 and impregnation liquid B1.
[0041] Example 6 provides a temperature-resistant, wear-resistant, self-lubricating lining material, comprising the following components: polytetrafluoroethylene fabric, pre-impregnation liquid A5 and impregnation liquid B1.
[0042] The test method is as follows:
[0043] Tensile performance test: This type of heat-resistant, wear-resistant, self-lubricating liner material is injection molded into a standard specimen with a specimen size of 115mm×10mm×4mm, and tested in accordance with GB / T1040-2006 "Test Method for Tensile Properties of Plastics".
[0044] Thermal conductivity test: This type of heat-resistant, wear-resistant, self-lubricating lining material is injection molded into a standard sample with a size of 300mm×300mm×20mm. The test is carried out in accordance with GB / T10294-2008 "Determination of Steady-State Thermal Resistance and Related Properties of Insulating Materials - Guarded Hot Plate Method".
[0045] Friction performance test: Use epoxy adhesive to bond the heat-resistant and wear-resistant self-lubricating lining material to the pin made of 45# steel, and cure it at room temperature for 24 hours under a pressure of 0.1MPa to obtain a friction test sample. Use a vertical universal friction and wear tester to test the friction performance of the prepared friction test sample. The friction and wear test conditions are: the friction test sample is worn against GCr15 stainless steel, the test load is 500N, the rotation speed is 12m / s, the room temperature air environment, the running time is 1h, and the friction coefficient and wear amount are the average values of 3 tests.
[0046] The test results are shown in Table 3, as follows:
[0047] Table 3 Performance test results list
[0048]
[0049]
[0050] Comparing Examples 1-2 with Examples 4-5, it can be seen that when the engineering resin and the nanofiller are within a reasonable range, the tensile properties, thermal conductivity and friction resistance of the heat-resistant and wear-resistant self-lubricating liner material prepared by the present invention are improved.
[0051] Comparison of Examples 1-2 and Comparative Example 1 shows that when the sulfonic acid dispersant provided by the present invention is used as the dispersant, the tensile properties, thermal conductivity and friction resistance of the heat-resistant and wear-resistant self-lubricating liner material prepared by the present invention are significantly improved.
[0052] Comparison between Examples 1-2 and 3 shows that the use of sulfonic acid dispersants and surfactants improves the tensile properties, thermal conductivity and friction resistance of the heat-resistant and wear-resistant self-lubricating liner material prepared by the present invention. Comparison between Examples 1-3 and 6 shows that when the sulfonic acid dispersants and secondary alcohol polyoxyethylene ethers are used in combination, the heat-resistant and wear-resistant self-lubricating liner material prepared by the present invention has a tensile strength of up to 50.3MPa, an elongation at break of 125%, a thermal conductivity of 3.65W / (m·K), a friction coefficient of 0.061, and a wear loss of 5.4mg, and has excellent mechanical properties, thermal conductivity and friction resistance.
[0053] In summary, the heat-resistant and wear-resistant self-lubricating gasket material provided by the present invention has excellent tensile properties, thermal conductivity and friction resistance. The use of sulfonic acid dispersant and secondary alcohol polyoxyethylene ether as the dispersion system makes the components of the heat-resistant and wear-resistant self-lubricating gasket material prepared by the present invention have good compatibility, thereby promoting the heat-resistant and wear-resistant self-lubricating gasket material to have good thermal conductivity and mechanical properties while maintaining low friction performance, further broadening the application of this type of material in high temperature, high load, and high friction conditions.
[0054] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A heat-resistant, wear-resistant, self-lubricating lining material, characterized in that: The raw materials for preparing the heat-resistant and wear-resistant self-lubricating lining material include polytetrafluoroethylene fabric, pre-impregnation liquid A and impregnation liquid B, wherein the pre-impregnation liquid A includes graphene and a sulfonic acid type dispersant; the impregnation liquid B includes polytetrafluoroethylene ultrafine powder, engineering resin and nano filler; the raw materials for preparing the sulfonic acid type dispersant include phthalic anhydride, diethylene glycol, maleic anhydride and sodium bisulfite.
2. The heat-resistant, wear-resistant, self-lubricating gasket material according to claim 1, characterized in that: The preparation method of the sulfonic acid type dispersant comprises the following steps: firstly subjecting phthalic anhydride and diethylene glycol to a ring-opening esterification reaction, using p-toluenesulfonic acid as a catalyst to obtain an intermediate 1, then reacting the obtained intermediate 1 with maleic anhydride under the condition of using p-toluenesulfonic acid as a catalyst to obtain an intermediate 2, adjusting the pH of the reaction liquid, and finally adding sodium bisulfite to carry out a sulfonation reaction to obtain the sulfonic acid type dispersant.
3. The heat-resistant, wear-resistant, self-lubricating lining material according to claim 1, characterized in that: The mass ratio of the engineering resin to the nanofiller in the impregnation liquid B is 1:(0.3-1).
4. The heat-resistant, wear-resistant, self-lubricating gasket material according to claim 1, characterized in that: The pre-dipping liquid A further comprises a surfactant, and the surfactant is a secondary alcohol polyoxyethylene ether.
5. The heat-resistant, wear-resistant, self-lubricating gasket material according to claim 1, characterized in that: The engineering resin includes one or more of phenolic resin, polyimide resin and epoxy resin.
6. The heat-resistant, wear-resistant, self-lubricating lining material according to claim 1, characterized in that: The nano filler comprises one or more of nano titanium dioxide, nano aluminum oxide and nano silicon dioxide.
7. The heat-resistant, wear-resistant, self-lubricating gasket material according to claim 1, characterized in that: The mass ratio of graphene to sulfonic acid dispersant in the pre-impregnation liquid A is 1:(0.5-1), and the mass ratio of polytetrafluoroethylene ultrafine powder to the total mass of engineering resin and nanofiller in the impregnation liquid B is 1:(0.5-0.9).
8. The heat-resistant, wear-resistant, self-lubricating gasket material according to claim 1, characterized in that: The raw materials for preparing the polytetrafluoroethylene fabric include aramid fiber and polytetrafluoroethylene fiber. The specification of the aramid fiber is 400-1000D filament, and the specification of the polytetrafluoroethylene fiber is 200-600D filament.
9. A method for preparing a heat-resistant, wear-resistant, self-lubricating lining material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: preparing polytetrafluoroethylene fabric, weaving aramid fiber as warp yarn and polytetrafluoroethylene fiber as weft yarn to obtain polytetrafluoroethylene fabric; S2: preparing pre-impregnation liquid A, mixing graphene and sulfonic acid dispersant, adding them to deionized water, and ultrasonicating for 40-60 minutes to obtain pre-impregnation liquid A for standby use; preparing impregnation liquid B, mixing polytetrafluoroethylene ultrafine powder, engineering resin and nanofiller, adding them to ethanol solution, and ultrasonicating for 40-60 minutes to obtain impregnation liquid B for standby use; S3: impregnating the polytetrafluoroethylene fabric prepared in S1 into the pre-impregnation liquid A for 60-180 minutes and then drying. After the above operation is repeated for several times, a modified polytetrafluoroethylene fabric is obtained; S4: Soak the modified polytetrafluoroethylene fabric in the impregnation liquid B, and repeatedly scrape and squeeze for 30-40 minutes to obtain an impregnated composite material; then, the impregnated composite material is compression molded to obtain a heat-resistant, wear-resistant, self-lubricating liner material.
10. The method for preparing a heat-resistant, wear-resistant, self-lubricating lining material according to claim 9, characterized in that: The compression molding process is performed under pressure conditions of 15-40 MPa, a temperature of 330-340° C., and a holding time of 1-4 h.
Citation Information
Cited By
Aramid rope conveying belt and preparation method thereof
CN120553318A
Aramid fiber rope conveyor belt and method of making same
CN120553318B
Sulfonated polyphenyl sulfone impregnated self-lubricating fabric composite material and preparation method thereof
CN121228537A
Glass fabric reinforced polytetrafluoroethylene functional gradient composite material, preparation method thereof, retainer and bearing
CN121608411A