Organosilicon paste for enhancing wear resistance and leveling property of coating and preparation method thereof

By using a combination of hydroxyl raw glue, polyether silicone oil and emulsifier treated with specific proportions and processes, silicone paste with ultra-large molecular weight is prepared, which solves the problem of the negative impact of traditional silicone paste increasing production costs and performance, and realizes the coating High performance and stability, suitable for a variety of coatings.

CN119039823APending Publication Date: 2024-11-29HANGZHOU SICAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411308164.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

While improving the performance of the coating, traditional silicone pastes increase production costs and may have negative effects on other properties, such as reducing adhesion or increasing drying time, and insufficient leveling and scratch resistance of the coating.

Method used

Using a combination of hydroxyl raw glue, polyether silicone oil and emulsifier, through specific proportions and processes, an organic silicon paste with super-large molecular weight is prepared to improve the wear resistance and leveling of the coating, reduce the addition amount and reduce production costs. .

Benefits of technology

It is achieved that the leveling and scratch resistance of the paint can be significantly improved in the case of very small amounts of addition, maintain or optimize other properties, improve the weather resistance and stability of the paint, and reduce production costs, and is suitable for a variety of paints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039823A_ABST
    Figure CN119039823A_ABST
Patent Text Reader

Abstract

The invention mainly relates to the technical field of coating performance enhancement, in particular to organic silicon paste for enhancing wear resistance and leveling property of a coating and a preparation method thereof, and the organic silicon paste comprises the following components in parts by weight: 60-80 parts of hydroxyl raw rubber, 5-15 parts of polyether silicone oil, 3-10 parts of an emulsifier and 10-30 parts of a water solvent. The organic silicon raw rubber with ultra-large molecular weight covers the surface of a base material or a coating and has very good wear resistance and scratch resistance, and the polyether silicone oil has good leveling property, so that the silicon paste with the two advantages can be obtained by adding the two components with excellent performance into the formula, and the weather resistance of the coating can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention mainly relates to the fields of "coating preparation technology", "organic silicon material preparation technology" and "coating performance enhancement technology", and specifically to an organosilicon paste for enhancing the wear resistance and leveling properties of coatings and a preparation method thereof. Background Art

[0002] Paint has been widely used. According to its use, it can be divided into interior paint, exterior paint, wood paint and metal paint. Painting the surface of walls or appliances can greatly protect them and increase their service life.

[0003] In the field of coating preparation technology, silicone materials are widely used in the preparation of coatings due to their excellent weather resistance, heat resistance, electrical insulation, hydrophobicity and other properties. Among them, silicone paste is a commonly used silicone material, which can improve the leveling, wear resistance and scratch resistance of coatings by changing its formula and process parameters. However, in practical applications, traditional silicone pastes often require a large amount of addition to achieve the desired effect, which not only increases production costs, but may also affect other properties of the coating.

[0004] The existing solutions in the prior art are mainly to improve the performance of silicone paste by changing the formula and process parameters of silicone paste, such as increasing the proportion of hydroxyl raw rubber, or adjusting the type and amount of emulsifier, so as to reduce the amount of silicone paste added in the coating. In addition, there are some solutions to improve the performance of the coating by adding other functional materials, such as nano-scale fillers.

[0005] Although the prior art has provided some solutions, these solutions still have some problems and shortcomings. First, while existing silicone pastes improve performance, they often increase their production costs, which is an important consideration for paint manufacturers. Secondly, while existing silicone pastes improve paint performance, they may have a negative impact on other properties, such as reducing the adhesion of the paint, or increasing the drying time of the paint. In addition, most of the paints on the market currently have poor leveling and are easily rubbed or scratched off, so it is very important to increase the leveling and scratch resistance of the paint itself.

[0006] In view of this, the present invention provides an organosilicon paste for enhancing the wear resistance and leveling properties of a coating and a preparation method thereof. Summary of the invention

[0007] The object of the present invention is to provide an organic silicone paste for enhancing the wear resistance and leveling properties of a coating and a preparation method thereof in view of the deficiencies of the prior art.

[0008] In order to solve the above technical problems, the following technical solutions are adopted: The organic silicone paste used to enhance the wear resistance and leveling property of the coating comprises the following components in parts by weight: 60-80 parts of hydroxyl rubber; Polyether silicone oil 5-15 parts; Emulsifier 3-10 parts; 10-30 parts of water solvent.

[0009] A further improvement based on the technical solution is that the molecular weight range of the hydroxyl raw rubber is 50w-80w.

[0010] A further improvement based on the technical solution is that the emulsifier includes one or more of secondary alcohol polyoxyethylene ethers, straight-chain primary alcohol polyoxyethylenes and alkylphenol polyoxyethylenes.

[0011] A further improvement based on the technical solution is that the viscosity of the polyether silicone oil ranges from 1000 to 10000 cst.

[0012] The present invention proposes another technical solution: a method for preparing an organic silicone paste for enhancing the wear resistance and leveling property of a coating, characterized in that: the raw materials prepared include hydroxyl raw rubber, polyether silicone oil, emulsifier and water solvent; S1. At room temperature, add hydroxyl rubber, polyether silicone oil and emulsifier into a reaction vessel and stir to mix evenly, wherein the ratio of hydroxyl rubber, polyether silicone oil and emulsifier is (60-80): (5-15): (3-10); S2. Add an appropriate amount of aqueous solvent to start dispersion and make the mixture into a paste. During this process, the paste mixture reaches a predetermined particle size; S3. Add the remaining water solvent to dilute and obtain the silicone paste.

[0013] A further improvement based on the technical solution is that in step S1, the time for stirring and mixing the raw materials evenly is 2-3 hours.

[0014] A further improvement based on the technical solution is that in step S2, the stirring time after adding the first portion of water is 0.5-3 hours.

[0015] A further improvement based on the technical solution is that in step S3, the dilution time using water solvent is 10-60 minutes.

[0016] The above technical solution has the following beneficial effects: In the present invention, since the organic silicone rubber with ultra-large molecular weight has very good wear resistance and scratch resistance when covered on the surface of the substrate or the coating, and the polyether silicone oil has good leveling properties, adding these two components with excellent performance into the formula can obtain a silicone paste with both advantages, and can increase the weather resistance of the coating.

[0017] In the present invention, since the ultra-large molecular weight hydroxyl raw rubber cannot be emulsified by an emulsifier, polyether silicone oil is added thereto as a diluent, and the polyether silicone oil itself also has leveling properties.

[0018] Advantages and beneficial effects of the present invention: Compared with existing products, the silicone paste of the present invention can be added to the coating as a coating additive. The coating adding a very small amount of this product can show excellent leveling and wear and scratch resistance. The silicone paste of the present invention will not have a negative impact on other properties while improving the performance of the coating, such as not reducing the adhesion of the coating, and will not increase the drying time of the coating. The silicone paste of the present invention has excellent stability during storage and transportation, and will not have problems such as stratification and precipitation, which greatly improves its application effect in the coating and has higher practical value compared to the prior art. In general, the silicone paste of the present invention has significant advantages in improving coating performance, reducing production costs, and ensuring product quality stability.

[0019] In summary, the waterproofing agent has a wide range of applications and can be applied to a variety of different coatings. The product of the present invention has stable properties, good storage resistance, low raw material cost, low production equipment requirements, and is easy to industrially mass produce. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The properties of the silicone paste prepared in Examples 1 and 2 of the present invention are shown in FIG.

[0021] Figure 2 This is the effect of scratching blank wood paint.

[0022] Figure 3 The figure is a scratching effect diagram of the coating after adding the organic silicone paste of the present invention.

[0023] Figure 4 This is a comparison chart of the surface sliding friction coefficient when the silicone paste prepared in Example 1 of the present invention is added to wood coating. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below through the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0025] The organic silicone paste used to enhance the wear resistance and leveling property of the coating comprises the following components in parts by weight: 60-80 parts of hydroxyl rubber; Polyether silicone oil 5-15 parts; Emulsifier 3-10 parts; 10-30 parts of water solvent.

[0026] As a further illustration of this embodiment, the molecular weight of the hydroxylated raw rubber is in the range of 50w-80w.

[0027] As a further illustration of this embodiment, the emulsifier includes one or more of secondary alcohol polyoxyethylene ethers, linear primary alcohol polyoxyethylenes and alkylphenol polyoxyethylenes.

[0028] As a further illustration of this embodiment, the viscosity of the polyether silicone oil ranges from 1000 to 10000 cst.

[0029] The present invention proposes another technical solution: a method for preparing an organic silicone paste for enhancing the wear resistance and leveling property of a coating, characterized in that: the raw materials prepared include hydroxyl raw rubber, polyether silicone oil, emulsifier and water solvent; S1. At room temperature, add hydroxyl rubber, polyether silicone oil and emulsifier into a reaction vessel and stir to mix evenly, wherein the ratio of hydroxyl rubber, polyether silicone oil and emulsifier is (60-80): (5-15): (3-10); S2. Add an appropriate amount of aqueous solvent to start dispersion and make the mixture into a paste. During this process, the paste mixture reaches a predetermined particle size; S3. Add the remaining water solvent to dilute and obtain the silicone paste.

[0030] As a further illustration of this embodiment, in step S1, the time for stirring and mixing the raw materials evenly is 2-3 hours.

[0031] As a further illustration of this embodiment, in step S2, the stirring time after adding the first portion of water is 0.5-3 hours.

[0032] As a further illustration of this embodiment, in step S3, the dilution time using the water solvent is 10-60 minutes.

[0033] The present invention selects hydroxyl rubber and polyether silicone oil of specific molecular weight as main raw materials, wherein the molecular weight of hydroxyl rubber is 50w or 80w, and the viscosity of polyether silicone oil is in the range of 1000-3000 cst. This selection can make the silicone paste have good leveling and wear resistance and scratch resistance, and at the same time, the huge molecular weight of hydroxyl rubber can give the coating better weather resistance.

[0034] In a reaction vessel, hydroxyl rubber, polyether silicone oil and emulsifier (such as secondary alcohol polyoxyethylene ether emulsifier) ​​are mixed and stirred for 2-2.5 hours in a certain proportion to make them evenly mixed. This treatment method can make the hydroxyl rubber and polyether silicone oil fully mixed and improve the performance of the silicone paste.

[0035] A certain amount of water is added to the mixed raw materials, and the dispersion stirring is started to make the mixture into a paste. In this process, the performance of the silicone paste can be further improved by controlling the particle size range to 10-20um.

[0036] After the paste mixture reaches a predetermined particle size, a certain amount of water is added to dilute it to obtain the final silicone paste product. This treatment method can make the concentration of the silicone paste moderate and easy to use.

[0037] The prepared silicone paste is tested for scratch resistance, leveling performance and stability to verify its performance and stability. This testing method can ensure the effect of the silicone paste in actual application.

[0038] The silicone paste synthesized by using hydroxyl raw rubber, polyether silicone oil, emulsifier, etc. can not only give the coating good leveling, wear resistance and scratch resistance when added to the coating, but also give the coating better weather resistance due to the huge molecular weight of hydroxyl raw rubber.

[0039] The organosilicon paste of the present invention can reduce the amount of the paste added to the coating while improving the leveling and scratch resistance of the coating, thereby reducing production costs and meeting the cost-effectiveness requirements of coating manufacturers. Secondly, the organosilicon paste of the present invention will not have a negative impact on other coating properties, such as adhesion and drying time, so while ensuring the original performance of the coating, it can also improve its performance and meet consumers' demand for high-performance coatings. Finally, the organosilicon paste of the present invention has excellent stability and will not have problems such as stratification and precipitation during storage and transportation. Therefore, it is more convenient to use and meets the requirements of coating manufacturers for product quality and stability.

[0040] The present invention will be further described below by the following examples. Example 1

[0041] Weigh 140g of hydroxyl raw rubber with a molecular weight of 50w, 10g of polyether silicone oil, and 3g of secondary alcohol polyoxyethylene ether emulsifier into a reaction container and stir for 2 hours to mix evenly. Then add 20g of water to the reaction container, start dispersing and stirring to mix evenly to form a paste. When the particle size reaches about 10um, add 11g of water to dilute to obtain the final product. (Properties such as Figure 1 The first figure is shown in Figure 9.11). Example 2

[0042] Weigh 140g of hydroxyl raw rubber with a molecular weight of 80w, 18g of polyether silicone oil, and 9g of secondary alcohol polyoxyethylene ether emulsifier into a reaction container and stir for 2 hours to mix evenly. Then add 13g of water to the reaction container, start dispersing and stirring to mix evenly to form a paste. When the particle size reaches about 15um, add 20g of water to dilute to obtain the final product. (Properties such as Figure 1 (as shown in the second figure 9.20).

[0043] Experiment 1: Scratch resistance Test method: The same tester uses the same hard object (such as fingernails, comb teeth, etc.) to scrape back and forth on the paint film surface of each experimental group, creating defects as much as possible within 5 seconds, and then observes the state of the paint film.

[0044] Note: The hard object should not come into contact with the substrate when scraping, otherwise use another object as a scraper.

[0045] Result judgment: The group without added feel agent is rated as level 1 (lowest), and the unscratched state is rated as level 5 (highest). The severity of damage caused by scratches is used as the basis for relative grade scoring.

[0046] in conclusion: The paint film with the silicone paste added can achieve a scratch resistance level of 4, while the blank paint film without the silicone paste has a scratch resistance level of 1, which proves that the silicone paste can significantly improve the scratch resistance of the paint film.

[0047] Experiment 2: Leveling performance Test Method 1) See Figure 2 , Figure 3 and Figure 4 , place the cured sample horizontally at an appropriate position on the friction coefficient tester, ensuring that the slider is always on the paint film surface during the test.

[0048] 2) Place the slider on the paint film and click on it for testing. Repeat the test 5 times for each sample. Data that differ from the average value by more than 5% should be discarded, and the average value of the retained data should be taken as the output result.

[0049] Result determination The leveling performance is expressed by the change in the dynamic friction coefficient of the paint film surface after adding the feel agent.

[0050] Conclusion: Compared with the blank group without adding the silicone paste, the friction coefficient of the paint film with the addition of this product decreased by about 32%.

[0051] Experiment 3: Stability test The silicone paste product was placed in a centrifuge, the speed was set to 3000 rpm, and the test was conducted for 30 minutes. No white carbon black was precipitated, indicating that the white carbon black dispersion was stable.

[0052] The silicone paste product was placed in a freeze-thaw box, set at -20 degrees Celsius, and cycled for 5 groups over 48 hours. No stratification was observed, indicating good freeze-thaw stability.

[0053] In summary, the organic silicone paste of the present invention is suitable for various coatings including wood coatings, can give the coatings obvious leveling and scratch resistance, and has certain weather resistance. The organic silicone paste of the present invention has excellent stability and storage resistance.

[0054] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.

Claims

1. Organic silicone paste used to enhance the wear resistance and leveling properties of coatings, characterized by: The composition comprises the following components in parts by weight: 60-80 parts of hydroxyl rubber; Polyether silicone oil 5-15 parts; Emulsifier 3-10 parts; 10-30 parts of water solvent.

2. The organic silicone paste for enhancing the wear resistance and leveling properties of coatings according to claim 1, characterized in that: The molecular weight of the hydroxyl raw rubber is in the range of 50w-80w.

3. The organic silicone paste for enhancing the wear resistance and leveling properties of coatings according to claim 1, characterized in that: The emulsifier includes one or more of secondary alcohol polyoxyethylene ethers, linear primary alcohol polyoxyethylenes and alkylphenol polyoxyethylenes.

4. The organic silicone paste for enhancing the wear resistance and leveling properties of coatings according to claim 1, characterized in that: The viscosity of the polyether silicone oil ranges from 1000 to 10000 cst.

5. A method for preparing an organic silicone paste for enhancing the wear resistance and leveling properties of a coating as claimed in any one of claims 1 to 4, characterized in that: The prepared raw materials include hydroxyl raw rubber, polyether silicone oil, emulsifier and water solvent; S1. At room temperature, add hydroxyl rubber, polyether silicone oil and emulsifier into a reaction vessel and stir to mix evenly, wherein the ratio of hydroxyl rubber, polyether silicone oil and emulsifier is (60-80): (5-15): (3-10); S2. Add an appropriate amount of aqueous solvent to start dispersion and make the mixture into a paste. During this process, the paste mixture reaches a predetermined particle size; S3. Add the remaining water solvent to dilute and obtain the silicone paste.

6. The method for preparing the organic silicone paste for enhancing the wear resistance and leveling properties of coatings according to claim 5, characterized in that: In step S1, the time for stirring and mixing the raw materials evenly is 2-3 hours.

7. The method for preparing the organic silicone paste for enhancing the wear resistance and leveling properties of coatings according to claim 5, characterized in that: In step S2, the stirring time after adding the first portion of water is 0.5-3 hours.

8. The method for preparing the organic silicone paste for enhancing the wear resistance and leveling properties of coatings according to claim 5, characterized in that: In step S3, the dilution time using the water solvent is 10-60 minutes.