Organic-inorganic hybrid photochromic coating and preparation method thereof

By introducing polyvinylpyrrolidone into the photochromic coating, forming a polymer network and reacting with the tungsten oxide precursor, the problem of insufficient transparency and discoloration sensitivity of the photochromic coating in the prior art is solved, and high Transparency, instant response and rapid fading effects significantly improve the energy efficiency and visible sunlight comfort of the building.

CN119039846AActive Publication Date: 2024-11-29SOUTHEAST UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411156967.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing organic-inorganic hybrid photochromic coating based on WO3 has insufficient transparency and dimming range, and the discoloration effect is not sensitive enough, and the fading time is long, which affects the energy efficiency and visible sunlight comfort of the building.

Method used

By introducing polyvinylpyrrolidone into the photochromic coating, forming a polymer and reacting with the tungsten oxide precursor, a photochromic coating with amorphous WO3 nanodots highly dispersed in the polymer network is prepared, using polymers The hydrogen bond density and nitrogen content in it increase the light response speed and color discoloration depth, achieving high transparency, instantaneous light response and rapid fading effects.

Benefits of technology

Significantly improves the transparency and color change depth of the coating, achieves 96% visible light transparency, fast response and dark blue color change, can effectively absorb infrared light, reduce indoor energy consumption, and maintain good resistance to aging and environment under 50 cycles. stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039846A_ABST
    Figure CN119039846A_ABST
Patent Text Reader

Abstract

The invention discloses an organic-inorganic hybrid photochromic coating and a preparation method thereof.The preparation method comprises the following steps that 1, a monomer A, a monomer B and a monomer C are subjected to random copolymerization under the action of photo-initiated free radicals, and a high-molecular polymer of a three-dimensional network structure is formed; wherein the monomer A is an amide compound containing an olefin functional group; the monomer B is a fluorine-containing acrylate compound; the monomer C is an imidazole compound containing an olefin functional group; (2) dissolving a high-molecular polymer and polyvinylpyrrolidone into an organic solvent, uniformly mixing, adding a tungsten oxide precursor into the solution, and reacting at room temperature; and (3) coating a glass substrate with the reacted mixed solution, and drying to obtain the photochromic coating. In the prepared coating, the amorphous WO3 nanodots are highly dispersed in a polymer network, and the particle size of the amorphous WO3 nanodots is not higher than 1.03 nm. The photochromic coating is high in transparency (the photochromic coating is transparent before and after discoloration), has instantaneous light response and rapid fading effects, is large in discoloration degree, and also has good environmental stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an organic-inorganic hybrid photochromic coating and also to a method for preparing the photochromic coating. Background Art

[0002] As the global temperature continues to rise, the energy consumption for building cooling has been further increased. Therefore, it is crucial to improve the energy efficiency of buildings and reduce carbon emissions. By adjusting the light transmittance of windows and controlling the input of solar energy in buildings, the energy efficiency and visible daylight comfort of buildings can be effectively improved.

[0003] Photochromic (PC) smart windows with simple structures that can modulate light without external energy input have great development potential. Tungsten oxide undergoes charge transfer under external light, and the electrons in the material jump from the valence band to the conduction band to form conductive or non-conductive tungsten oxide, which causes color changes. Because of its rapid response to light and excellent reversibility, it has become one of the most intensively studied inorganic photochromic materials.

[0004] In the process of preparing organic-inorganic hybrid photochromic coatings based on WO3, due to the different characteristics of organic polymers and inorganic photochromic materials, they will affect each other's transparency during the hybridization or composite process, resulting in low transparency of the final material. In addition, WO3 is easy to grow in a directional manner to form a larger crystalline structure, so the prepared photochromic material has problems such as low transparency and narrow dimming range. Tungsten oxide changes color and fades through redox reactions, which will be affected by organic polymer chains. The color change effect is not sensitive enough and it takes a long time to complete the color change. The material has low oxygen permeability, resulting in a long fading time. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide an organic-inorganic hybrid photochromic coating, which has high transparency (transparent before and after color change), instantaneous light response and rapid fading effect, and a large degree of color change, and also has good environmental stability; another purpose of the present invention is to provide a method for preparing the above-mentioned photochromic coating.

[0006] Technical solution: The method for preparing the organic-inorganic hybrid photochromic coating of the present invention comprises the following steps:

[0007] (1) Monomer A, monomer B and monomer C are randomly copolymerized under the action of photoinitiated free radicals to form a high molecular polymer with a three-dimensional network structure; wherein monomer A is an amide compound containing an olefin functional group; monomer B is a fluorine-containing acrylate compound; and monomer C is an imidazole compound containing an olefin functional group;

[0008] (2) dissolving the polymer and polyvinyl pyrrolidone in an organic solvent, mixing well, adding a tungsten oxide precursor, and reacting at room temperature;

[0009] The introduction of polyvinyl pyrrolidone can, on the one hand, increase the hydrogen bond density between polymer molecules, thereby improving the mechanical strength of the coating; on the other hand, it can increase the nitrogen content in the polymer, promote the transfer speed of electrons and protons under light excitation, and greatly improve the light response speed and color change depth of amorphous WO3 nanodots;

[0010] (3) coating the mixed solution after the reaction on a glass substrate and drying it to obtain a photochromic coating.

[0011] Wherein, in step (1), the monomer A is one of acrylamide, N-isopropylacrylamide, N,N-dimethylacrylamide or acryloylmorpholine; the monomer B is one of trifluoroethyl acrylate, hexafluoroisopropyl acrylate, hexafluorobutyl acrylate, dodecafluoroheptyl acrylate, trifluoroethyl methacrylate, hexafluoroisopropyl methacrylate, hexafluorobutyl methacrylate or dodecafluoroheptyl methacrylate; and the monomer C is one of N-vinylimidazole, 1-allylimidazole or 1-(3-butene-1-yl)-1H-imidazole.

[0012] Wherein, in step (1), the amount of monomer A added is 20% to 30% of the total molar amount of monomer A, monomer B and monomer C; the amount of monomer B added is 40% to 50% of the total molar amount of monomer A, monomer B and monomer C; the amount of monomer C added is 20% to 30% of the total molar amount of monomer A, monomer B and monomer C.

[0013] Wherein, in step (1), the photoinitiator is one of 907, TPO, 184, 1173, DETX, ITX, 369 or 2599; the amount of the photoinitiator added is 1 to 1.5% of the total molar amount of monomer A, monomer B and monomer C.

[0014] Wherein, in step (2), the organic solvent is N,N-dimethylformamide.

[0015] Wherein, in step (2), the average molecular weight of the polyvinyl pyrrolidone is 3000-30000; and the mass ratio of polyvinyl pyrrolidone to the high molecular polymer is 0.05-0.2:1.

[0016] Wherein, in step (2), the mass concentration of the high molecular weight polymer in the solution is 0.4 to 0.6 g / mL.

[0017] Wherein, in step (2), the tungsten oxide precursor is one of phosphotungstic acid, tungsten chloride, sodium tungstosilicate, sodium calcium tungstosilicate, sodium tungstate or sodium potassium tungstate; and the added amount of the tungsten oxide precursor is 10-20% of the total mass of the high molecular weight polymer and polyvinyl pyrrolidone.

[0018] Wherein, in step (2), the drying temperature is 100-120° C., and the drying time is not less than 24 hours.

[0019] In the photochromic coating prepared by the above method, amorphous WO3 nanodots are highly dispersed in the polymer network, and the particle size of the amorphous WO3 nanodots is not higher than 1.03 nm.

[0020] The photochromic coating of the present invention is colorless and transparent. The amorphous WO3 nanodots absorb sunlight to trigger electron transitions, resulting in valence changes, so that the entire coating is colored. In a dark environment, it quickly turns colorless and transparent.

[0021] The photochromic coating of the present invention converts the WO3 nanodots from an oxidized state to a reduced state under the excitation of sunlight, so that the entire coating is colored; after the coating is colored, it can effectively reduce the absorption of infrared light indoors, thereby achieving the effect of energy saving and emission reduction. Specifically, as the irradiation time of sunlight increases, the coating changes from light blue to dark blue, and can absorb a wider range of infrared light. The absorbed infrared light is converted into heat energy on the surface of the coating and dissipated into the outside air with the natural wind, thereby saving the energy consumption required for indoor cooling.

[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: on the one hand, the polymer in the coating of the present invention can limit the growth and aggregation of WO3, and in situ grow amorphous tungsten oxide nanodots with a size of about 1 nm in the polymer network, and by making the amorphous WO3 nanodots highly dispersed in the polymer network (no crystal structure will be formed under high dispersion), the transparency of the coating is greatly improved, and the visible light transmittance of the coating in a transparent state reaches 96%; at the same time, since the amorphous WO3 nanodots have a small size and a large specific surface area, the activity and speed of the redox reaction can be highly enhanced, thereby effectively enhancing the light response speed and the color change depth of the coating; on the other hand, the polymer can also greatly promote the transfer speed of electrons and protons under light excitation and the penetration effect of oxygen, further making the coating have a large degree of color change while having instantaneous light response and rapid fading effect; the coating of the present invention also has the advantages of good aging resistance and environmental stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a high-resolution transmission electron microscopy image of the photochromic coating in Example 1 of the present invention;

[0024] Figure 2 is the XRD spectrum of the photochromic coating in Example 1 of the present invention;

[0025] Figure 3 The infrared absorption spectra of the photochromic coating in Example 1 of the present invention before and after changing color under sunlight irradiation for 20 minutes;

[0026] Figure 4 The effect diagram of the photochromic coating in Example 1 of the present invention before and after the color change after being irradiated with sunlight for 20 minutes;

[0027] Figure 5 This is a schematic diagram of the change in visible light transmittance of the photochromic coating in Example 1 of the present invention during 30 minutes of sunlight irradiation;

[0028] Figure 6 This is a schematic diagram of changes in visible light transmittance during the fading of the photochromic coating in a dark environment for 4 hours in Example 1 of the present invention;

[0029] Figure 7 The surface temperature monitoring curve of the blank glass and the coated glass when the photochromic coating in Example 1 of the present invention is irradiated by sunlight;

[0030] Figure 8 The indoor temperature monitoring curves of blank glass and photochromic coated glass in real environment.

[0031] Fig. 9 This is a data graph of 50 cycles of coloring and fading of the photochromic coating in Example 1 of the present invention;

[0032] Fig.10 The data graphs are of the basic light transmittance and glass transition temperature of the coatings with different contents of PVP introduced in Examples 1, 8, 9 and 10 of the present invention;

[0033] Fig.11 The diagrams are the visible light adjustment ranges of the coatings with different PVP contents introduced in Examples 1, 8, and 9 of the present invention, and the color change spectrum of the coating in Example 1 after being irradiated with a 365nm ultraviolet lamp for different time periods;

[0034] Fig.12 It is the polymer network structure of the photochromic coating of the present invention. DETAILED DESCRIPTION

[0035] Example 1

[0036] The method for preparing the organic-inorganic hybrid photochromic coating of the present invention comprises the following steps:

[0037] (1) N-vinyl imidazole (723 μL, 8 mmol), 4-acryloylmorpholine (1509.8 μL, 12 mmol), trifluoroethyl methacrylate (2306.1 μL, 20 mmol) and photoinitiator 1173 (61 μL, 0.4 mmol) were mixed and stirred at room temperature for 20 min to obtain a mixed solution; the mixed solution was poured into a 0.3 mm thick silica gel mold and irradiated under a 35 W ultraviolet light (365 nm) with an appearance size of 180 mm*140 mm*120 mm for 10 minutes to obtain a polymer PVH;

[0038] (2) 5 g of the polymer PVH prepared in step (1) and 0.75 g of polyvinyl pyrrolidone (PVP) were dissolved in 12 mL of N,N-dimethylformamide (DMF), and stirred at room temperature for 20 to 30 min; 575 mg of phosphotungstic acid was added to the solution, and the mixture was stirred at room temperature for 1 h to obtain a mixed solution;

[0039] (3) Pour the mixed solution of step (2) onto the glass substrate on the surface of the coater, set the liquid film thickness to 400 μm, the glass substrate temperature to 40° C., dry for 2 h, and then transfer to a 100° C. oven for drying for 24 h to obtain an organic-inorganic hybrid photochromic coating with a thickness of 100 μL.

[0040] Example 2

[0041] The preparation method of Example 2 is basically the same as that of Example 1, except that in step (1), the molar ratio of N-vinylimidazole, 4-acryloylmorpholine and trifluoroethyl methacrylate is 3:2:5.

[0042] Example 3

[0043] The preparation method of Example 3 is basically the same as that of Example 1, except that in step (1), the molar ratio of N-vinylimidazole 4-acryloylmorpholine to trifluoroethyl methacrylate is 3:3:4.

[0044] Example 4

[0045] The preparation method of Example 4 is substantially the same as that of Example 1, with the only difference being that in step (1), 4-acryloylmorpholine is replaced with one of N,N-dimethylacrylamide, acrylamide or N-isopropylacrylamide.

[0046] Example 5

[0047] The preparation method of Example 5 is basically the same as that of Example 1, with the only difference being that in step (1), trifluoroethyl methacrylate is replaced by one of trifluoroethyl acrylate, hexafluoroisopropyl acrylate, hexafluorobutyl acrylate, dodecafluoroheptyl acrylate, hexafluorobutyl methacrylate, hexafluoroisopropyl methacrylate or dodecafluoroheptyl methacrylate.

[0048] Example 6

[0049] The preparation method of Example 6 is basically the same as that of Example 1, with the only difference being that in step (1), N-vinylimidazole is replaced by 1-allylimidazole or 1-(3-butene-1-yl)-1H-imidazole.

[0050] Example 7

[0051] The preparation method of Example 7 is basically the same as that of Example 1, with the only difference being that in step (2), phosphotungstic acid is replaced by one of tungsten chloride, sodium / calcium tungstosilicate or sodium / potassium tungstate.

[0052] Example 8

[0053] The preparation method of Example 8 is basically the same as that of Example 1, with the only difference being that in step (2), the mass ratio of PVP to PVH is 0.05:1, and the tungsten oxide precursor accounts for 10% of the total mass of the polymer.

[0054] Example 9

[0055] The preparation method of Example 9 is basically the same as that of Example 1, with the only difference being that in step (2), the mass ratio of PVP to PVH is 0.1:1, and the tungsten oxide precursor accounts for 10% of the total mass of the polymer.

[0056] Example 10

[0057] The preparation method of Example 10 is basically the same as that of Example 1, with the only difference being that in step (2), the mass ratio of PVP to PVH is 0.2:1, and the tungsten oxide precursor accounts for 10% of the total mass of the polymer.

[0058] pass Figure 1 High resolution transmission electron microscopy images and Figure 2 The XRD characterization of the coating revealed the internal microstructure of the polymer. The data showed that WO3 did not form crystals inside the polymer (no lattice fringes and crystallization characteristic peaks of WO3). The particle size of tungsten oxide was measured to be 1.03nm through high-resolution transmission electron microscopy.

[0059] pass Figure 3It shows that the coating has a wider range of infrared light absorption after color change, which is the basis for giving the coating the building cooling and energy-saving performance. The coating has a wider range of infrared light absorption after color change, which can reduce the infrared light absorption inside the building, thereby slowing down the temperature rise in the room.

[0060] pass Figures 5-6 It can be seen that when the photochromic coating of Example 1 is placed under sunlight for 20 minutes, the color of the coating gradually darkens, the transmittance decreases significantly, the coating absorbs infrared light, and the surface temperature of the coating begins to rise; the coating begins to fade spontaneously in the dark state, and the transparency gradually increases; the visible light (400nm~800nm) transmittance of the photochromic coating is adjusted in the range of 96% to 4.8%.

[0061] The coating of Example 1 can achieve an instantaneous light response speed, reaching the optimal speed in 20 minutes. The degree of discoloration is characterized by the transmittance of the UV-visible spectrum. After irradiation under a 365nm UV lamp for 20 minutes, the visible light transmittance of the coating drops to 4.8% (ultraviolet light excitation causes discoloration, changing the visible light transmittance of the coating), indicating that the degree of discoloration is deep.

[0062] The photochromic coating of Example 1 is used to adjust the transmittance of sunlight and thus adjust the indoor temperature. A model room with the photochromic coating glass of Example 1 and blank glass is placed outdoors in a real environment to monitor the indoor temperature for 80 hours. Figure 8 It can be seen that the coating can effectively reduce the entry of infrared light into the room and slow down the rise of indoor temperature after changing color. Fig. 9 It can be seen that the coating of the present invention has good aging resistance and environmental stability. After 50 cycles, the light transmittance and color change ability of the coating remain basically unchanged.

Claims

1. A method for preparing an organic-inorganic hybrid photochromic coating, characterized in that: The steps include: (1) Monomer A, monomer B and monomer C are randomly copolymerized under the action of photoinitiated free radicals to form a high molecular polymer with a three-dimensional network structure; wherein monomer A is an amide compound containing an olefin functional group; monomer B is a fluorine-containing acrylate compound; and monomer C is an imidazole compound containing an olefin functional group; (2) dissolving the polymer and polyvinyl pyrrolidone in an organic solvent, mixing them evenly, and then adding a tungsten oxide precursor to the solution to react at room temperature; (3) coating the reaction mixture on a glass substrate by spraying, laminating, blade coating or inkjet printing, and drying to obtain a photochromic coating.

2. The method for preparing a photochromic coating according to claim 1, characterized in that: In step (1), the monomer A is one of acrylamide, N-isopropylacrylamide or N,N-dimethylacrylamide; the monomer B is one of trifluoroethyl acrylate, hexafluoroisopropyl acrylate, hexafluorobutyl acrylate, dodecafluoroheptyl acrylate, trifluoroethyl methacrylate, hexafluoroisopropyl methacrylate, hexafluorobutyl methacrylate or dodecafluoroheptyl methacrylate; and the monomer C is one of N-vinylimidazole, 1-allylimidazole or 1-(3-butene-1-yl)-1H-imidazole.

3. The method for preparing the photochromic coating according to claim 1, characterized in that: In step (1), the amount of monomer A added is 20% to 30% of the total molar amount of monomer A, monomer B and monomer C; the amount of monomer B added is 40% to 50% of the total molar amount of monomer A, monomer B and monomer C; the amount of monomer C added is 20% to 30% of the total molar amount of monomer A, monomer B and monomer C.

4. The method for preparing a photochromic coating according to claim 1, characterized in that: In step (1), the photoinitiator is one of 907, TPO, 184, 1173, DETX, ITX, 369 or 2599; the amount of the photoinitiator added is 1 to 1.5% of the total molar amount of monomer A, monomer B and monomer C.

5. The method for preparing a photochromic coating according to claim 1, characterized in that: In step (2), the organic solvent is N,N-dimethylformamide.

6. The method for preparing a photochromic coating according to claim 1, characterized in that: In step (2), the average molecular weight of the polyvinyl pyrrolidone is 3000-30000; the mass ratio of polyvinyl pyrrolidone to the high molecular polymer is 0.05-0.2:

1.

7. The method for preparing a photochromic coating according to claim 1, characterized in that: In step (2), the mass concentration of the high molecular weight polymer in the solution is 0.4 to 0.6 g / mL.

8. The method for preparing a photochromic coating according to claim 1, characterized in that: In step (2), the tungsten oxide precursor is one of phosphotungstic acid, tungsten chloride, sodium tungstosilicate, sodium calcium tungstosilicate, sodium tungstate or sodium potassium tungstate; the amount of the tungsten oxide precursor added is 10-20% of the total mass of the high molecular weight polymer and polyvinyl pyrrolidone.

9. The method for preparing a photochromic coating according to claim 1, characterized in that: In step (2), the drying temperature is 100-120° C. and the drying time is not less than 24 hours.

10. The photochromic coating prepared by the preparation method according to claim 1, characterized in that: In the coating, amorphous WO3 nanodots are highly dispersed in the polymer network, and the particle size of the amorphous WO3 nanodots is no greater than 1.03 nm.

Citation Information

Patent Citations

  • Organic-inorganic composite electrochromic film and preparation method thereof

    CN102352109A

  • Nano-composite optothermal response system, resin material and smart glass

    CN105713238A

  • Repeatable electrochromic colorful photonic crystal film structure and preparation method thereof

    CN116449621A

  • Coated material

    US5063114A