Stainless steel pipe applied to maritime work and machining process

By coating the surface of stainless steel pipes with a corrosion-resistant coating, the problems of corrosion and microbial erosion of stainless steel pipes in marine engineering are solved, thereby improving corrosion resistance and mechanical properties, and extending service life through self-healing microcapsules.

CN119039855APending Publication Date: 2024-11-29CHANGSHU HEXIN STAINLESS STEEL TUBE PROD CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411284302.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Stainless steel pipes are susceptible to corrosion and microbial attack in marine engineering, which affects their service life.

Method used

A corrosion-resistant coating is applied to the surface of stainless steel pipes. The coating consists of water-based epoxy resin, self-healing microcapsules, inorganic nanofillers, and a curing agent. The corrosion resistance is improved by enhancing the compatibility and stability of the components.

Benefits of technology

It significantly improves the corrosion resistance and mechanical properties of stainless steel pipes, extends their service life, and enhances the stability and durability of the coating by repairing cracked coatings through self-healing microcapsules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042669360000081
    Figure BDA0005042669360000081
Patent Text Reader

Abstract

The invention relates to a stainless steel pipe applied to maritime work and a machining process, the stainless steel pipe comprises a pipe body and a corrosion-resistant coating, the corrosion-resistant coating is obtained by coating the surface of the pipe body with a corrosion-resistant coating, and the corrosion-resistant coating comprises waterborne epoxy resin, filler, a self-repairing microcapsule component, a dispersing agent, a flatting agent and a curing agent; the water-borne epoxy resin comprises epoxy resin emulsion, an organic silicon compound and inorganic nano filler. The effect of improving the corrosion resistance of the stainless steel pipe is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of stainless steel pipes, and in particular to a stainless steel pipe and a processing technology used in marine engineering. Background Art

[0002] Marine engineering refers to new construction, reconstruction and expansion projects that are built for the purpose of developing, utilizing, protecting and restoring marine resources, and the main body of the project is located on the sea side of the coastline.

[0003] Stainless steel pipes also play an important role in the transportation of marine engineering. When stainless steel comes into contact with seawater, it will corrode the steel pipes. At the same time, microorganisms in the ocean will also corrode the stainless steel pipes, affecting the service life of the stainless steel pipes. Summary of the invention

[0004] In order to improve the corrosion resistance of stainless steel pipes, the present application provides a stainless steel pipe and a processing technology for marine engineering.

[0005] The present application provides a stainless steel pipe and processing technology for offshore engineering, which adopts the following technical solutions: In the first aspect, the present application provides a stainless steel pipe for offshore engineering, which adopts the following technical solution: A stainless steel pipe used in marine engineering comprises a pipe body and a corrosion-resistant coating. The corrosion-resistant coating is obtained by coating the corrosion-resistant coating on the surface of the pipe body. The corrosion-resistant coating comprises a water-based epoxy resin, a filler, a self-repairing microcapsule component, a dispersant, a leveling agent and a curing agent; the water-based epoxy resin comprises an epoxy resin emulsion, an organosilicon composite and an inorganic nanofiller.

[0006] By adopting the above technical scheme, after the corrosion-resistant coating is coated on the surface of the stainless steel pipe, a layer of corrosion-resistant coating is attached to the surface of the stainless steel pipe. The corrosion-resistant coating mainly uses water-based epoxy resin and self-healing microcapsules as the main body, wherein the water-based epoxy resin includes epoxy resin emulsion, silicone composite and inorganic nanofiller. After the epoxy resin emulsion is cured on the surface of the pipe body, it can play a good protective role on the pipe body, and at the same time has good mechanical properties and corrosion resistance, which effectively improves the corrosion resistance of the stainless pipe. At the same time, inorganic nanofillers are added, and the compatibility of each component in the system is improved through the action of the silicone composite, so that each component can be well dispersed in the micropores generated by the shrinkage of the water-based epoxy resin during the curing coating, further improving the stability of the corrosion-resistant coating, and improving the mechanical properties of the corrosion-resistant coating, so as to improve the long-term corrosion protection of the pipe body.

[0007] Preferably, the waterborne epoxy resin is prepared by the following method: The method comprises the following steps: mixing tetraethyl orthosilicate, anhydrous ethanol, a silane coupling agent and water, stirring the mixture, and reacting the mixture under an oil bath condition to obtain an organosilicon composite; mixing nano titanium nitride and nano silicon dioxide microspheres to obtain a nano composite; mixing the nano composite with a silane coupling agent, ethanol and water, stirring the mixture magnetically, and reacting the mixture under stirring condition; washing the mixture after centrifugation to obtain a product; dispersing the product in ethanol, adding the product to octadecyl methacrylate and azobisisobutyronitrile, heating the mixture, stirring the mixture, reacting the mixture, filtering the mixture, and drying the mixture to obtain an inorganic nano filler; mixing an epoxy resin emulsion, a wetting agent and a defoaming agent, adding titanium dioxide and precipitated barium sulfate, and stirring the mixture; after the system is defoamed, adding the organosilicon composite and the inorganic nano filler, and stirring the mixture to obtain a waterborne epoxy resin.

[0008] By adopting the above technical scheme, nano-titanium nitride and nano-silicon dioxide microspheres are compounded, and the surface of the nano-composite is modified so that a large number of active groups are connected to the surface of the nano-composite to improve the dispersibility and compatibility of the nano-composite in the system, so that the nano-composite can be more stably dispersed in the epoxy resin emulsion; the organic silicon composite obtained by combining tetraethyl orthosilicate, anhydrous ethanol and a silane coupling agent can form a silica sol, thereby reducing the phenomenon of the organic silicon composite hydrolyzing too quickly and becoming ineffective, further improving the stability and durability of the water-based epoxy resin, and being able to provide long-term protection for the pipeline body.

[0009] Preferably, the silane coupling agent includes γ-methacryloxypropyltrimethoxysilane.

[0010] By adopting the above technical scheme, γ-methacryloxypropyltrimethoxysilane is used as a silane coupling agent. On the one hand, when preparing an organic silicon composite, the turbidity of the system is improved, thereby improving the stability of the organic silicon composite. The groups in γ-methacryloxypropyltrimethoxysilane can undergo a cross-linking reaction with the molecules in ethyl orthosilicate, making the network structure of the organic silicon composite more compact and stable, thereby improving the overall mechanical properties of the corrosion-resistant coating; on the other hand, when preparing an inorganic nanofiller, γ-methacryloxypropyltrimethoxysilane can react with the hydroxyl groups on the surfaces of nano-silica microspheres and nano-titanium nitride under acidic conditions, so that the surface roughness of the nano-composite is modified, further improving the dispersibility and compatibility of the nano-composite in the system, thereby improving the stability of the corrosion-resistant coating.

[0011] Preferably, the mass ratio of the epoxy resin emulsion, the organosilicon composite and the inorganic nanofiller is 1:(0.11-0.13):0.08.

[0012] By adopting the above technical solution, the mass ratio of the epoxy resin emulsion, the organosilicon composite and the inorganic nanofiller is preferably within the above range, which can further improve the stability of the water-based epoxy resin.

[0013] Preferably, the self-repairing microcapsules include tung oil, toluene diisocyanate and polyvinyl alcohol.

[0014] By adopting the above technical solution, the coating formed by the epoxy resin emulsion will also crack after long-term use. After adding self-repairing microcapsules to the system, the cracked coating can be repaired, thereby improving the service life of the corrosion-resistant coating; tung oil is a natural material of sensible plant oils, and contains components such as linolenic acid, linoleic acid and oleic acid. The unsaturated double bonds in tung oil can react with O 2 A cross-linking reaction occurs and fills the cracks, effectively reducing the phenomenon of further cracking of the corrosion-resistant coating. Polyvinyl alcohol has good stability, and the self-healing microcapsules prepared by compounding with toluene diisocyanate can effectively improve the mechanical properties and durability of the corrosion-resistant coating.

[0015] Preferably, the self-repairing microcapsules are prepared by the following method: After tung oil and toluene diisocyanate are mixed, polyvinyl alcohol is added and uniformly dispersed to obtain tung oil emulsion, the tung oil emulsion is stirred in a water bath to obtain a suspension, the suspension is centrifuged, washed, and freeze-dried to obtain self-healing microcapsules.

[0016] Preferably, the curing agent includes 2-ethyl-4-methylimidazole.

[0017] By adopting the above technical solution, 2-ethyl-4-methylimidazole is used as a curing agent, and an addition reaction can occur between the N atom and the epoxy group, and then after cross-linking and curing, a stable corrosion-resistant coating is formed on the surface of the pipeline body.

[0018] Preferably, the mass ratio of the waterborne epoxy resin, the self-healing microcapsule component and the curing agent is 3.3:(0.24-0.28):1.

[0019] By adopting the above technical solution, the mass ratio between the water-based epoxy resin, the self-healing microcapsule component and the curing agent is preferably within the above range, which can further improve the stability of the corrosion-resistant coating of the system.

[0020] In a second aspect, the present application provides a processing technology for a stainless steel pipe applied to offshore engineering, which adopts the following technical solution: A processing technology for a stainless steel pipe applied to offshore engineering, comprising the following steps: The pipe body is preheated, and the corrosion-resistant coating is evenly coated on the surface of the pipe body and cured to form a layer of corrosion-resistant coating on the surface of the pipe body. After the curing is completed, the pipe body is cooled to obtain a stainless steel pipe product.

[0021] In summary, the present application includes at least one of the following beneficial technical effects: 1. After the corrosion-resistant coating is applied on the surface of the pipeline body, a layer of corrosion-resistant coating is formed. After the water-based epoxy resin is cured, it can provide good protection for the pipeline body, thereby improving the corrosion resistance of the pipeline body. Through the compatibility of the organic silicon composite and the improvement component, the inorganic nanofiller can be well dispersed in the micropores generated by the shrinkage of the water-based epoxy resin during the curing coating, so as to improve the overall stability of the corrosion-resistant coating and the mechanical properties of the corrosion-resistant coating, thereby improving the durability of the corrosion-resistant coating; 2. Using γ-methacryloxypropyltrimethoxysilane as a silane coupling agent, on the one hand, when preparing the silicone composite, the turbidity of the system is improved, thereby improving the stability of the silicone composite. The groups in γ-methacryloxypropyltrimethoxysilane can undergo cross-linking reactions with the molecules in ethyl orthosilicate, making the network structure of the silicone composite more compact and stable, thereby improving the overall mechanical properties of the corrosion-resistant coating; on the other hand, when preparing inorganic nanofillers, γ-methacryloxypropyltrimethoxysilane can react with the hydroxyl groups on the surface of nano-silica microspheres and nano-titanium nitride under acidic conditions to modify the surface roughness of the nano-composite, further improving the dispersibility and compatibility of the nano-composite in the system, thereby improving the stability of the corrosion-resistant coating.

[0022] 3. The self-healing microcapsules were prepared by combining tung oil, toluene diisocyanate and polyvinyl alcohol. When the epoxy resin emulsion coating cracked, the unsaturated double bonds in the tung oil could react with the O 2 A cross-linking reaction occurs to fill the cracks in the coating, reducing the phenomenon of further cracking of the coating, thereby further improving the stability and durability of the corrosion-resistant coating. DETAILED DESCRIPTION

[0023] The present application is further described in detail below with reference to the embodiments: Raw material description: All raw materials in the embodiment can be obtained commercially; the wetting agent is HY-4100 wetting agent, the defoaming agent is TEGO-8030 defoaming agent; the dispersant is 5040 dispersant; the leveling agent is BYK-378 leveling agent; the curing agent is 2-ethyl-4-methylimidazole (CAS No.: 931-36-2); the stainless tube is made of 400 stainless steel.

[0024] Example 1 Preparation of self-healing microcapsules: After mixing 13.5g of tung oil (CAS No.: 8001-20-5) and 6.75g of toluene diisocyanate (CAS No.: 26471-62-5), 225ml of 5wt% polyvinyl alcohol was added, and the mixture was homogenized and dispersed using a homogenizer for 5 minutes to obtain a tung oil emulsion. The tung oil emulsion was stirred at a speed of 300r / min for 3 hours in a water bath at 60°C to obtain a suspension. After centrifuging the suspension, it was washed with ethanol, frozen at -4°C for 12 hours, and then transferred to a freeze dryer and freeze-dried in a vacuum environment for 24 hours to obtain self-healing microcapsules.

[0025] Preparation of inorganic nanofillers: 15 g of nano titanium nitride and 15 g of nano silicon dioxide microspheres were mixed to obtain a nanocomposite, the nanocomposite was mixed with 5 g of silane coupling agent, 300 g of ethanol and 100 g of deionized water, magnetically stirred and acetic acid was used to adjust the pH value of the system to 4, then the temperature was raised to 60°C, the stirring condition was maintained for reaction for 2 h, and the product was washed with ethanol after centrifugation to obtain the product, the product was dispersed in 150 g of ethanol, 15 g of octadecyl methacrylate (CAS No.: 32360-05-7) and 0.25 g of azobisisobutyronitrile (CAS No.: 78-67-1) were added, the temperature was raised to 60°C, the reaction was stirred at a speed of 600 r / min for 2 h, and then filtered, and dried in a 45°C dryer at 60°C to obtain an inorganic nanofiller.

[0026] Preparation of silicone composites: After mixing 15.24 g of tetraethyl orthosilicate, 30.48 g of anhydrous ethanol, 30.48 g of silane coupling agent and 3.8 g of water, stir at 80 r / min for 3 min, then use hydrochloric acid to adjust the pH value of the system to 2, stir and react at 120 r / min for 6 h in an oil bath at 60°C to obtain an organosilicon composite.

[0027] Preparation of corrosion resistant coatings: After mixing 252.1 g of epoxy resin emulsion (CAS No.: 61788-97-4), 4 g of wetting agent and 2 g of defoaming agent, add 30 g of titanium dioxide and 15 g of precipitated barium sulfate, keep stirring at a speed of 1200 r / min for 1 hour, after the system is defoamed, add 27.73 g of silicone composite and 20.17 g of inorganic nanofiller, stir at a speed of 300 r / min for 45 minutes to obtain a water-based epoxy resin, mix 200 g of water-based epoxy resin, 14.55 g of self-healing microcapsule component, 5 g of dispersant, 4 g of leveling agent and 60.61 g of curing agent, stir at a speed of 300 r / min for 45 minutes to obtain a corrosion-resistant coating.

[0028] Preparation of stainless steel tube: Preheat the pipe body to 60°C, evenly apply the corrosion-resistant coating on the surface of the pipe body, maintain the temperature of 60°C, and cure for 2 hours to form a layer of corrosion-resistant coating on the surface of the pipe body. After curing, cool to 25°C to obtain a stainless steel pipe product.

[0029] In Example 1, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane (CAS No.: 2530-85-0).

[0030] Example 2 Preparation of self-healing microcapsules: After mixing 13.5g of tung oil and 6.75g of toluene diisocyanate, 225ml of 5wt% polyvinyl alcohol was added, and the mixture was homogenized and dispersed using a homogenizer for 5 minutes to obtain a tung oil emulsion. The tung oil emulsion was stirred at 300r / min for 3 hours in a water bath at 60°C to obtain a suspension. The suspension was centrifuged, washed with ethanol, frozen at -4°C for 12 hours, and then transferred to a freeze dryer and freeze-dried in a vacuum environment for 24 hours to obtain self-healing microcapsules.

[0031] Preparation of inorganic nanofillers: 15 g of nano titanium nitride and 15 g of nano silicon dioxide microspheres were mixed to obtain a nanocomposite, the nanocomposite was mixed with 5 g of silane coupling agent, 300 g of ethanol and 100 g of deionized water, magnetically stirred and acetic acid was used to adjust the pH value of the system to 4, then the temperature was raised to 60°C, the stirring condition was maintained for reaction for 2 h, and the product was washed with ethanol after centrifugation to obtain the product, the product was dispersed in 150 g of ethanol, 15 g of octadecyl methacrylate and 0.25 g of azobisisobutyronitrile were added, the temperature was raised to 60°C, the reaction was stirred at a speed of 600 r / min for 2 h, and then filtered, and dried in a 45°C dryer at 60°C to obtain an inorganic nanofiller.

[0032] Preparation of silicone composites: After mixing 15.24 g of tetraethyl orthosilicate, 30.48 g of anhydrous ethanol, 30.48 g of silane coupling agent and 3.8 g of water, stir at 80 r / min for 3 min, then use hydrochloric acid to adjust the pH value of the system to 2, stir and react at 120 r / min for 6 h in an oil bath at 60°C to obtain an organosilicon composite.

[0033] Preparation of corrosion resistant coatings: After mixing 247.93 g of epoxy resin emulsion, 4 g of wetting agent and 2 g of defoaming agent, add 30 g of titanium dioxide and 15 g of precipitated barium sulfate, keep stirring at a speed of 1200 r / min for 1 hour, after the system is defoamed, add 32.24 g of silicone composite and 19.83 g of inorganic nanofiller, stir at a speed of 300 r / min for 45 minutes to obtain a water-based epoxy resin, mix 240 g of water-based epoxy resin, 20.36 g of self-healing microcapsule component, 7 g of dispersant, 6 g of leveling agent and 72.73 g of curing agent, stir at a speed of 300 r / min for 45 minutes to obtain a corrosion-resistant coating.

[0034] Preparation of stainless steel tube: Preheat the pipe body to 60°C, evenly apply the corrosion-resistant coating on the surface of the pipe body, maintain the temperature of 60°C, and cure for 2 hours to form a layer of corrosion-resistant coating on the surface of the pipe body. After curing, cool to 25°C to obtain a stainless steel pipe product.

[0035] Example 3 Preparation of self-healing microcapsules: After mixing 13.5g of tung oil and 6.75g of toluene diisocyanate, 225ml of 5wt% polyvinyl alcohol was added, and the mixture was homogenized and dispersed using a homogenizer for 5 minutes to obtain a tung oil emulsion. The tung oil emulsion was stirred at 300r / min for 3 hours in a water bath at 60°C to obtain a suspension. The suspension was centrifuged, washed with ethanol, frozen at -4°C for 12 hours, and then transferred to a freeze dryer and freeze-dried in a vacuum environment for 24 hours to obtain self-healing microcapsules.

[0036] Preparation of inorganic nanofillers: 15 g of nano titanium nitride and 15 g of nano silicon dioxide microspheres were mixed to obtain a nanocomposite, the nanocomposite was mixed with 5 g of silane coupling agent, 300 g of ethanol and 100 g of deionized water, magnetically stirred and acetic acid was used to adjust the pH value of the system to 4, then the temperature was raised to 60°C, the stirring condition was maintained for reaction for 2 h, and the product was washed with ethanol after centrifugation to obtain the product, the product was dispersed in 150 g of ethanol, 15 g of octadecyl methacrylate and 0.25 g of azobisisobutyronitrile were added, the temperature was raised to 60°C, the reaction was stirred at a speed of 600 r / min for 2 h, and then filtered, and dried in a 45°C dryer at 60°C to obtain an inorganic nanofiller.

[0037] Preparation of silicone composites: After mixing 15.24 g of tetraethyl orthosilicate, 30.48 g of anhydrous ethanol, 30.48 g of silane coupling agent and 3.8 g of water, stir at 80 r / min for 3 min, then use hydrochloric acid to adjust the pH value of the system to 2, stir and react at 120 r / min for 6 h in an oil bath at 60°C to obtain an organosilicon composite.

[0038] Preparation of corrosion resistant coatings: After mixing 250g of epoxy resin emulsion, 4g of wetting agent and 2g of defoaming agent, add 30g of titanium dioxide and 15g of precipitated barium sulfate, keep stirring at 1200r / min for 1h, after the system is defoamed, add 30g of silicone composite and 20g of inorganic nanofiller, stir at 300r / min for 45min to obtain water-based epoxy resin, mix 220g of water-based epoxy resin, 17.33g of self-healing microcapsule component, 6g of dispersant, 5g of leveling agent and 66.67g of curing agent, stir at 300r / min for 45min to obtain corrosion-resistant coating.

[0039] Preparation of stainless steel tube: Preheat the pipe body to 60°C, evenly apply the corrosion-resistant coating on the surface of the pipe body, maintain the temperature of 60°C, and cure for 2 hours to form a layer of corrosion-resistant coating on the surface of the pipe body. After curing, cool to 25°C to obtain a stainless steel pipe product.

[0040] Example 4 Example 4 is based on Example 3. The difference between Example 4 and Example 3 is that in Example 4, when preparing the water-based epoxy resin, 260.87 g of epoxy resin emulsion, 18.26 g of organosilicon composite and 20.87 g of inorganic nanofiller are used.

[0041] Example 5 Example 5 is based on Example 3. The difference between Example 5 and Example 3 is that in Example 5, when preparing the water-based epoxy resin, 243.9 g of epoxy resin emulsion, 36.59 g of organosilicon composite and 19.51 g of inorganic nanofiller are used.

[0042] Example 6 Example 6 is based on Example 3. The difference between Example 6 and Example 3 is that in Example 6, the inorganic nanofiller is prepared by physically mixing silicon dioxide and titanium nitride in a mass ratio of 1:1.

[0043] Example 7 Example 7 is based on Example 3. The difference between Example 7 and Example 3 is that in Example 7, no nano titanium nitride is added to the inorganic nano filler.

[0044] Example 8 Example 8 is based on Example 3. The difference between Example 8 and Example 3 is that in Example 8, no nano-silicon dioxide is added to the inorganic nano-filler.

[0045] Example 9 Example 9 is based on Example 3. In Example 9, when preparing the self-repairing microcapsule component, polyvinyl alcohol is replaced by deionized water.

[0046] Example 10 Example 10 is based on Example 3, and the silane coupling agent in Example 10 is γ-aminopropyltriethoxysilane (CAS No.: 919-30-2).

[0047] Comparative Example 1 Comparative Example 1 is based on Example 3, and in Comparative Example 1, the self-repairing microcapsules are replaced with an equal amount of tung oil.

[0048] Comparative Example 2 Comparative Example 2 is based on Example 3, but no organosilicon composite is added in Comparative Example 2.

[0049] Comparative Example 3 Comparative Example 3 is based on Example 3, and no inorganic nanofiller is added in Comparative Example 3.

[0050] Performance testing The following performance tests were performed on the samples of Examples 1-10 and Comparative Examples 1-3: (1) Corrosion resistance test The sample was placed in a corrosion solution (including 12wt% nitric acid, 3wt% hydrofluoric acid, and 0.5wt% sodium chloride) and the corrosion rate test was performed at room temperature. Each sample was tested three times, the average value was taken, and the test results were filled in Table 1.

[0051] (2) Impact resistance test The tensile strength and impact toughness of the steel strip were tested in accordance with GB / T 229-2007 Impact test method for metal materials. Each sample was tested three times and the test results were filled in Table 1.

[0052] (3) Self-healing test After making a cross cut on the coating surface of the sample, it was immersed in a 3.5% NaCl solution by mass and the impact resistance test was performed again after 3 days. Each sample was tested three times, the average value was taken, and the test results were filled in Table 1; the cross cut length was 40 mm, the width was 2 mm, and the depth was 2 mm.

[0053] Table 1 Performance test results of samples of Examples 1-10 and Comparative Examples 1-3 Data analysis Combined with Table 1, it can be seen that the corrosion rates in Examples 1-3 are all 4.32 mm / a or less, indicating that the stainless steel pipes prepared in the present application have good corrosion resistance; the impact toughness of Examples 1-3 is all 240 J or more, indicating that the stainless steel pipes prepared in the present application have good impact resistance; the repair efficiency of Examples 1-3 is all 74.49% or more, indicating that the stainless steel pipes prepared in the present application have good self-repairing properties.

[0054] In Example 4 and Example 5, when preparing the water-based epoxy resin, the ratios among the epoxy resin emulsion, the silicone composite and the inorganic nanofiller are not within the range defined in the present application. When the content of the silicone composite is too much, the content of the silane coupling agent in the system is too much, which dilutes the epoxy resin emulsion, thereby reducing the coating stability of the epoxy resin emulsion on the pipeline body and reducing the coating uniformity. When the content of the silicone composite is too little, the overall viscosity of the water-based epoxy resin is difficult to be further improved, and the bonding effect between the components is reduced. At the same time, the proportion of inorganic nanofillers increases, and too much inorganic nanofillers agglomerate in the system, thereby affecting the overall stability of the system. Therefore, the performance of Example 4 and Example 5 is reduced.

[0055] In Example 6, the inorganic nanofiller is only physically mixed, and the untreated nano titanium nitride and nano silicon dioxide are difficult to disperse evenly in the system and agglomerate, which affects the overall stability of the waterborne epoxy resin. Therefore, various properties in Example 6 are reduced.

[0056] In Examples 7 and 8, a single nanofiller was used in the preparation of inorganic nanofillers. A single nanofiller is difficult to synergistically improve the hydrophobicity and mechanical properties of the system, and it is also difficult to further improve the overall binding performance of the system. Therefore, the comprehensive performance of Examples 7 and 8 is reduced.

[0057] In Example 9, when preparing the self-healing microcapsule component, polyvinyl alcohol was replaced with deionized water. The overall stability of the self-healing microcapsule system was difficult to be further improved, and the particle size uniformity was difficult to improve, and it was difficult to disperse evenly in the system. Therefore, the performance of Example 9 was reduced.

[0058] In Example 10, the silane coupling agent is γ-aminopropyltriethoxysilane, which produces a large amount of silanol during hydrolysis, causing the cross-linking condensation between Si-OH to be too fast, thereby affecting the overall stability of the system.

[0059] In Comparative Example 1, the self-repairing microcapsules were replaced with an equal amount of tung oil. The uncoated tung oil was easily oxidized in the system, causing the tung oil to deactivate quickly. After the deactivated corrosion-resistant coating cracked, it was difficult to repair it again.

[0060] In Comparative Example 2, no silicone composite is added, which makes it difficult to improve the overall viscosity of the epoxy resin emulsion. At the same time, the connection effect between the components in the system is difficult to promote, and the bonding performance with the pipeline body is also reduced, so the performance in Comparative Example 2 is reduced.

[0061] In Comparative Example 3, no inorganic nanofiller is added. It is difficult to further improve the mechanical properties of the system without inorganic nanofiller, and it is difficult to improve the connection performance in the system, so the performance of Comparative Example 3 is reduced.

[0062] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of ​​the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A stainless steel pipe used in marine engineering, characterized by: It includes a pipeline body and a corrosion-resistant coating. The corrosion-resistant coating is obtained by coating the corrosion-resistant coating on the surface of the pipeline body. The corrosion-resistant coating includes water-based epoxy resin, filler, self-repairing microcapsule component, dispersant, leveling agent and curing agent; the water-based epoxy resin includes epoxy resin emulsion, silicone composite and inorganic nanofiller.

2. The stainless steel pipe for offshore engineering according to claim 1, characterized in that: The waterborne epoxy resin is prepared by the following method: The method comprises the following steps: mixing tetraethyl orthosilicate, anhydrous ethanol, a silane coupling agent and water, stirring the mixture, and reacting the mixture under an oil bath condition to obtain an organosilicon composite; mixing nano titanium nitride and nano silicon dioxide microspheres to obtain a nano composite; mixing the nano composite with a silane coupling agent, ethanol and water, stirring the mixture magnetically, and reacting the mixture under stirring condition; washing the mixture after centrifugation to obtain a product; dispersing the product in ethanol, adding the product to octadecyl methacrylate and azobisisobutyronitrile, heating the mixture, stirring the mixture, reacting the mixture, filtering the mixture, and drying the mixture to obtain an inorganic nano filler; mixing an epoxy resin emulsion, a wetting agent and a defoaming agent, adding titanium dioxide and precipitated barium sulfate, and stirring the mixture; after the system is defoamed, adding the organosilicon composite and the inorganic nano filler, and stirring the mixture to obtain a waterborne epoxy resin.

3. The stainless steel pipe for offshore engineering according to claim 1, characterized in that: The silane coupling agent includes γ-methacryloxypropyltrimethoxysilane.

4. The stainless steel pipe for offshore engineering according to claim 3, characterized in that: The mass ratio of the epoxy resin emulsion, the organosilicon composite and the inorganic nanofiller is 1:(0.11-0.13):0.

08.

5. The stainless steel pipe for offshore engineering according to claim 1, characterized in that: The self-repairing microcapsules include tung oil, toluene diisocyanate and polyvinyl alcohol.

6. The stainless steel pipe for offshore engineering according to claim 5, characterized in that: The self-repairing microcapsules are prepared by the following method: After tung oil and toluene diisocyanate are mixed, polyvinyl alcohol is added and uniformly dispersed to obtain tung oil emulsion, the tung oil emulsion is stirred in a water bath to obtain a suspension, the suspension is centrifuged, washed, and freeze-dried to obtain self-healing microcapsules.

7. The stainless steel pipe for offshore engineering according to claim 1, characterized in that: The curing agent includes 2-ethyl-4-methylimidazole.

8. The stainless steel pipe for offshore engineering according to claim 1, characterized in that: The mass ratio of the waterborne epoxy resin, the self-repairing microcapsule component and the curing agent is 3.3:(0.24-0.28):

1.

9. A processing technology for the stainless steel pipe used for offshore engineering according to claim 1, characterized in that: The steps include: The pipe body is preheated, and the corrosion-resistant coating is evenly coated on the surface of the pipe body and cured to form a layer of corrosion-resistant coating on the surface of the pipe body. After the curing is completed, the pipe body is cooled to obtain a stainless steel pipe product.

Citation Information

Patent Citations

  • Corrosion-resistant high-adhesive-force water-based metal paint

    CN104893499A

  • Preparation method of nanometer titanium nitride modified polyurethane paint

    CN107603451A

  • Self-repairing microcapsule, preparation method and application method thereof

    CN111298729A

  • Anticorrosive waterborne epoxy self-repairing coating for petroleum casing and preparation method and application of same

    CN112662272A

  • Condenser pipe inner cavity surface treatment process

    CN114958153A