Alkali-resistant self-adhesive vapor-proof coiled material for passive house

By using combined materials such as aluminum foil surface layer, modified asphalt layer and modified alumina in the steam insulation coil in the passive room, the problem of low steam insulation performance of the steam insulation coil is solved, and the water vapor diffusion resistance value is significantly improved and Water impermeable properties extend the service life of the building.

CN119039896AActive Publication Date: 2024-11-29HEBEI YUYANGZELI WATERPROOF MATERIAL
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411243455.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-29
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The steam insulation coils in the passive house have low vapor insulation performance and are easy to permeate, resulting in a decrease in the performance of the insulation material, mold and corrosion, affecting the overall performance and service life of the building.

Method used

The alkali-resistant self-adhesive steam insulation coil is used to use aluminum foil surface layer, modified asphalt layer, tire base layer and isolation layer film. By adjusting the swelling ratio of low-density polyethylene, the pores and cracks of the modified asphalt layer are reduced and water vapor diffusion is increased. Resistance value and modified alumina as adsorption filler enhance the water vapor adsorption capacity.

Benefits of technology

It significantly improves the water vapor diffusion resistance value and water impermeability of the steam insulation coil material, enhances alkali resistance, and extends the service life of the building.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of vapor-proof coiled materials, and provides an alkali-resistant self-adhesive vapor-proof coiled material for a passive house, which sequentially comprises an aluminum foil surface layer, a modified asphalt layer, a tire base layer, a self-adhesive layer and an isolating layer film from top to bottom, the modified asphalt layer comprises the following raw materials in parts by weight: 90-100 parts of 70 # asphalt, 12-15 parts of an asphalt modifier, 35-45 parts of filler, 9-10 parts of an antioxidant and 6-8 parts of a stabilizer; the asphalt modifier is prepared from SBS and low-density polyethylene, and the mass ratio of the SBS to the low-density polyethylene is 5: (1-3). By means of the technical scheme, the problems that in the prior art, a vapor-proof coiled material is low in vapor-proof performance and prone to water permeation are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vapor insulation coiled materials, and in particular to an alkali-resistant self-adhesive vapor insulation coiled material for a passive house. Background Art

[0002] Passive houses, or passive ultra-low energy buildings, are built by adopting advanced energy-saving design concepts and technical means, so that the building can maintain comfortable indoor temperature, humidity and air quality by relying only on its own thermal insulation performance and efficient heat recovery ventilation system, without relying on traditional active heating and cooling equipment. In today's construction field, passive houses are increasingly attracting widespread attention as a highly efficient and energy-saving building form. However, the construction of passive houses places higher requirements on building materials. In passive houses, the control of water vapor is crucial. Since passive houses have good thermal insulation performance, once water vapor enters the interior of the building structure, it is difficult to dissipate, which can easily lead to problems such as reduced performance of insulation materials, mold, and corrosion, thereby affecting the overall performance and service life of the building. Therefore, the development of an alkali-resistant self-adhesive vapor insulation membrane for passive houses with high vapor insulation performance and impermeable performance is an urgent problem to be solved. Summary of the invention

[0003] The invention provides an alkali-resistant self-adhesive steam-insulating coiled material for a passive house, which solves the problems of low steam-insulating performance and easy water permeability of the steam-insulating coiled material in the related art.

[0004] The technical scheme of the present invention is as follows: The present invention provides an alkali-resistant self-adhesive vapor insulation coil for a passive house, which comprises an aluminum foil surface layer, a modified asphalt layer, a tire base layer, a self-adhesive layer and an isolation layer membrane from top to bottom, wherein the modified asphalt layer comprises the following component raw materials in parts by weight: 90-100 parts of No. 70 asphalt, 12-15 parts of asphalt modifier, 35-45 parts of filler, 9-10 parts of antioxidant, and 6-8 parts of stabilizer; The asphalt modifier consists of SBS and low-density polyethylene, and the mass ratio of SBS to low-density polyethylene is 5:1-3.

[0005] As a further technical solution, the low-density polyethylene consists of a first low-density polyethylene and a second low-density polyethylene, and the first low-density polyethylene and the second low-density polyethylene have different melt expansion ratios.

[0006] In the present invention, the pores and cracks of the modified asphalt layer are reduced by adjusting the melt expansion ratio of the low-density polyethylene, thereby improving the water vapor diffusion resistance value and the water-impermeable performance of the vapor barrier coiled material.

[0007] As a further technical solution, the melt expansion ratio of the first low-density polyethylene is 0.87, the melt expansion ratio of the second low-density polyethylene is 1.8, and the mass ratio of the first low-density polyethylene to the second low-density polyethylene is 1:1-2.

[0008] As a further technical solution, the filler includes one or more of talc, alumina, and montmorillonite.

[0009] As a further technical solution, when the filler is alumina, the alumina is modified alumina.

[0010] As a further technical solution, the modifier of the modified alumina is 3-hydroxyphenylphosphorylpropionic acid.

[0011] As a further technical solution, the preparation steps of the modified alumina include: dissolving 3-hydroxyphenylphosphoryl propionic acid, adding alumina to disperse evenly, filtering and drying to obtain the modified alumina.

[0012] In the present invention, modified alumina is added as an adsorption filler to enhance the filler's ability to adsorb water vapor, thereby further improving the water vapor diffusion resistance value and water-impermeable performance of the vapor barrier coil.

[0013] As a further technical solution, the tire base layer is a glass fiber tire.

[0014] As a further technical solution, the antioxidant includes one or more of antioxidant 1098, antioxidant 697, and antioxidant 3114.

[0015] As a further technical solution, the stabilizer includes one or both of zinc stearate and calcium stearate.

[0016] The present invention also provides a method for preparing an alkali-resistant self-adhesive steam insulation coil for a passive house, comprising the following steps: S1. Weigh the raw material of the modified asphalt layer and melt it to obtain the modified asphalt layer; S2. Arrange the aluminum foil surface layer, modified asphalt layer, tire base layer, self-adhesive layer and isolation layer film in sequence, and after roller extrusion and cooling, obtain the alkali-resistant self-adhesive steam-insulating coiled material.

[0017] As a further technical solution, the self-adhesive layer is self-adhesive rubber asphalt, and the isolation layer film is a polyethylene film.

[0018] The working principle and beneficial effects of the present invention are: In the present invention, aluminum foil is used as the surface layer to prevent alkaline substances from contacting other materials inside the coil, thereby enhancing the alkali resistance of the vapor barrier coil. SBS and low-density polyethylene are used as composite modifiers to make the surface of the modified asphalt layer more dense, reduce the presence of tiny pores and cracks, and thus improve the vapor barrier and water-impermeable properties of the vapor barrier coil. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In the following examples and comparative examples: SBS: Model D1102; The first low-density polyethylene: melt expansion ratio is 0.87, density is 0.924g / cm 3 ; Second low-density polyethylene: melt expansion ratio is 1.8, density is 0.917g / cm 3 ; Aluminum foil surface layer: thickness 0.1mm; Self-adhesive layer: self-adhesive rubber asphalt 0.3mm; Isolation layer film: polyethylene film, thickness 0.2mm; Tire base: glass fiber, 0.5mm; Alkali-resistant self-adhesive steam barrier membrane: size is 10m×1m×1.6mm.

[0021] Example 1 A method for preparing an alkali-resistant self-adhesive steam insulation coil for a passive house comprises the following steps: S1. Weigh 95 parts of No. 70 asphalt, 10.8 parts of SBS, 1.2 parts of first low-density polyethylene, 35 parts of aluminum oxide, 9 parts of antioxidant 1098, and 6 parts of zinc stearate, heat to 170°C, melt and stir for 1 hour to obtain a modified asphalt layer; S2. Arrange the aluminum foil surface layer, modified asphalt layer, tire base layer, self-adhesive layer and isolation layer film in sequence, and after roller extrusion and cooling, obtain the alkali-resistant self-adhesive steam-insulating coiled material.

[0022] Example 2 A method for preparing an alkali-resistant self-adhesive steam insulation coil for a passive house comprises the following steps: S1. Weigh 95 parts of No. 70 asphalt, 11.7 parts of SBS, 1.3 parts of the first low-density polyethylene, 40 parts of talcum powder, 9.5 parts of antioxidant 697, and 7 parts of zinc stearate, heat to 175°C, melt-stir for 45 minutes, and obtain a modified asphalt layer; S2. Arrange the aluminum foil surface layer, modified asphalt layer, tire base layer, self-adhesive layer and isolation layer film in sequence, and after roller extrusion and cooling, obtain the alkali-resistant self-adhesive steam-insulating coiled material.

[0023] Example 3 A method for preparing an alkali-resistant self-adhesive steam insulation coil for a passive house comprises the following steps: S1. Weigh 100 parts of No. 70 asphalt, 13.5 parts of SBS, 1.5 parts of first low-density polyethylene, 45 parts of montmorillonite, 10 parts of antioxidant 3114, and 8 parts of calcium stearate, heat to 180°C, and melt-stir for 30 minutes to obtain a modified asphalt layer; S2. Arrange the aluminum foil surface layer, modified asphalt layer, tire base layer, self-adhesive layer and isolation layer film in sequence, and after roller extrusion and cooling, obtain the alkali-resistant self-adhesive steam-insulating coiled material.

[0024] Example 4 Compared with Example 1, Example 4 is different in that 10.8 parts of SBS and 1.2 parts of the first low-density polyethylene are replaced by 10 parts of SBS and 2 parts of the first low-density polyethylene.

[0025] Example 5 Compared with Example 1, Example 5 is different in that 10.8 parts of SBS and 1.2 parts of the first low-density polyethylene are replaced by 7.5 parts of SBS and 4.5 parts of the first low-density polyethylene.

[0026] Example 6 Compared with Example 1, Example 6 is different in that 10.8 parts of SBS and 1.2 parts of the first low-density polyethylene are replaced by 6 parts of SBS and 6 parts of the first low-density polyethylene.

[0027] Example 7 Compared with Example 5, the difference of Example 7 is that 4.5 parts of the first low-density polyethylene are replaced by an equal amount of the second low-density polyethylene.

[0028] Example 8 Compared with Example 5, Example 8 is different in that 4.5 parts of the first low-density polyethylene are replaced by 3 parts of the first low-density polyethylene and 1.5 parts of the second low-density polyethylene.

[0029] Example 9 Compared with Example 5, Example 9 is different in that 4.5 parts of the first low-density polyethylene are replaced by 2.25 parts of the first low-density polyethylene and 2.25 parts of the second low-density polyethylene.

[0030] Example 10 Compared with Example 5, Example 10 is different in that 4.5 parts of the first low-density polyethylene are replaced by 1.5 parts of the first low-density polyethylene and 3 parts of the second low-density polyethylene.

[0031] Embodiment 11 Compared with Example 5, Example 11 is different in that 4.5 parts of the first low-density polyethylene are replaced by 1 part of the first low-density polyethylene and 3.5 parts of the second low-density polyethylene.

[0032] Example 12 Compared with Example 10, the difference of Example 12 is that the alumina is replaced by an equal amount of modified alumina; Preparation of modified alumina: Weigh 8 parts of 3-hydroxyphenylphosphorylpropionic acid, dissolve it in 40 parts of ethanol, add 64 parts of alumina, disperse it ultrasonically for 1 hour, filter it, and dry it at 70°C to obtain modified alumina.

[0033] Comparative Example 1 Compared with Example 1, Comparative Example 1 is different in that only SBS is added.

[0034] Comparative Example 2 Compared with Example 1, Comparative Example 2 is different in that only the first low-density polyethylene is added.

[0035] The alkali-resistant self-adhesive steam-insulating coiled materials prepared in Examples 1 to 12 and Comparative Examples 1 to 2 were tested according to the following method: 1. Water vapor diffusion resistance value: According to the test method specified in GB / T 17146-2015 "Test method for water vapor permeability of building materials and their products", the water vapor diffusion resistance value of the test sample is tested.

[0036] 2. Waterproofness: According to the test method specified in GB / T 328.10-2007 "Test methods for building waterproof membranes Part 10: Waterproofness of bitumen and polymer waterproof membranes", select method B to test the water-proofness of the sample under a pressure of 0.2MPa for 30 minutes.

[0037] The test results are shown in the following table: Table 1 Performance test results of alkali-resistant self-adhesive steam barrier coils prepared in Examples 1 to 12 and Comparative Examples 1 to 2

[0038] Compared with Comparative Examples 1 and 2, Examples 1 to 6 simultaneously added SBS and the first low-density polyethylene. As a result, the water vapor diffusion resistance values ​​and water impermeability of Examples 1 to 6 were better than those of Comparative Examples 1 and 2, indicating that SBS and the first low-density polyethylene played a synergistic role and could improve the vapor barrier performance and water impermeability of the alkali-resistant self-adhesive vapor barrier coil. In Examples 1 and 4 to 6, SBS and the first low-density polyethylene were added in different mass ratios. As a result, the water vapor diffusion resistance values ​​of Examples 4 and 5 were better than those of Examples 1 and 6, indicating that when the mass ratio of SBS to the first low-density polyethylene was 5:1 to 3, the obtained alkali-resistant self-adhesive vapor barrier coil had better vapor barrier performance.

[0039] Compared with Examples 5 and 7, Examples 8 to 11 simultaneously added the first low-density polyethylene and the second low-density polyethylene. As a result, the water vapor diffusion resistance values ​​of Examples 8 to 11 were better than those of Examples 5 and 7, indicating that the first low-density polyethylene and the second low-density polyethylene played a synergistic role and could improve the vapor barrier performance of the alkali-resistant self-adhesive vapor barrier coil. In Examples 8 to 11, the first low-density polyethylene and the second low-density polyethylene were added in different mass ratios. As a result, the water vapor diffusion resistance values ​​of Examples 9 and 10 were better than those of Examples 9 and 11, indicating that when the mass ratio of the first low-density polyethylene to the second low-density polyethylene was 1:1 to 2, the obtained alkali-resistant self-adhesive vapor barrier coil had better vapor barrier performance.

[0040] Compared with Example 10, Example 12 adds modified alumina. As a result, the water vapor diffusion resistance value of Example 12 is better than that of Example 10, indicating that the addition of modified alumina can improve the vapor barrier performance of the alkali-resistant self-adhesive vapor barrier membrane.

[0041] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An alkali-resistant self-adhesive steam insulation coil for passive houses, characterized in that: From top to bottom, it includes an aluminum foil surface layer, a modified asphalt layer, a tread base layer, a self-adhesive layer and an isolation layer membrane. The modified asphalt layer includes the following component raw materials in parts by weight: 90-100 parts of No. 70 asphalt, 12-15 parts of asphalt modifier, 35-45 parts of filler, 9-10 parts of antioxidant, and 6-8 parts of stabilizer; the asphalt modifier is composed of SBS and low-density polyethylene, and the mass ratio of SBS to low-density polyethylene is 5:1-3.

2. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 1, characterized in that: The low-density polyethylene consists of a first low-density polyethylene and a second low-density polyethylene, and the first low-density polyethylene and the second low-density polyethylene have different melt expansion ratios.

3. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 2, characterized in that: The melt expansion ratio of the first low-density polyethylene is 0.87, the melt expansion ratio of the second low-density polyethylene is 1.8, and the mass ratio of the first low-density polyethylene to the second low-density polyethylene is 1:1-2.

4. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 1, characterized in that: The filler includes one or more of talc, alumina and montmorillonite.

5. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 4, characterized in that: When the filler is alumina, the alumina is modified alumina.

6. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 5, characterized in that: The modifier of the modified alumina is 3-hydroxyphenylphosphorylpropionic acid.

7. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 4, characterized in that: The preparation steps of the modified alumina include: dissolving 3-hydroxyphenylphosphoryl propionic acid, adding alumina to disperse evenly, filtering and drying to obtain the modified alumina.

8. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 1, characterized in that: The tire base layer is a glass fiber tire.

9. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 1, characterized in that: The antioxidant includes one or more of antioxidant 1098, antioxidant 697, and antioxidant 3114.

10. The alkali-resistant self-adhesive vapor insulation coil for passive houses according to claim 1, characterized in that: The stabilizer includes one or both of zinc stearate and calcium stearate.

Citation Information

Patent Citations

  • Self-adhesive modified asphalt waterproof coiled material coating material, preparation method thereof and aluminum foil surface self-adhesive asphalt waterproof coiled material special for passive buildings

    CN110746929A