High-modulus acrylate pressure-sensitive adhesive, preparation method thereof and polaroid protective film
By introducing monomers with specific structures into the acrylate copolymer, high-modulus acrylate pressure-sensitive adhesive is formed, and the problems of insufficient adhesion, durability, antistatic characteristics and high-speed peeling force in the prior art are solved, achieving high efficiency polarizer protection effect.
Patent Information
- Application Number
- CN202411294715.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art is difficult to provide an acrylic pressure sensitive adhesive with excellent adhesion, durability, antistatic properties, exhaust properties and high-speed peeling force, which is used to protect polarizers, especially in high-temperature aging and high-speed peeling force. .
Using high-modulus acrylate pressure-sensitive adhesive made of acrylate copolymer, antistatic agent, antioxidant and curing agent, the acrylate copolymer is introduced by introducing alkyl groups, hydroxyl groups, carboxyl groups, amide groups, alkylamino groups, Monomers with ethoxy and siloxane structures are prepared by two-stage solution radical polymerization to form polymers with covalent bonds, hydrogen bonds and van der Waals forces, enhancing the cohesion and modulus of the polymer.
The energy storage modulus of high-modulus acrylate pressure-sensitive adhesive at 100Hz reaches 1~50×105Pa, with excellent durability and low high-speed peeling force, and is verified by FT-IR, XRD and TEM characterization. The intermolecular interaction force meets the requirements of the polarizer protective film.
Smart Images

Figure BDA0005045585200000101 
Figure BDA0005045585200000102 
Figure BDA0005045585200000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pressure-sensitive adhesives, and in particular to a high-modulus acrylic pressure-sensitive adhesive and a preparation method thereof, and a polarizer protective film. Background Art
[0002] Polarizers are indispensable raw materials in the manufacturing process of LCD and OLED panels. At present, China's domestic LCD and OLED panel production capacity accounts for 62.1% and 29.4% of the world respectively. From the perspective of production capacity concentration, BOE, CSOT, and HKC account for more than 90% of China's LCD production capacity, while BOE alone has the largest OLED production capacity. In 2023, China's domestic demand for polarizers will reach about 380 million square meters, accounting for about 65% of the world.
[0003] In order to prevent the polarizer from being contaminated or damaged during transportation and storage, a protective film needs to be attached to its surface. This protective film is usually made of acrylic pressure-sensitive adhesive. During the panel assembly process, the protective film must be torn off from the surface of the polarizer. Static electricity will be generated when it is torn off. Static electricity will damage the display on the one hand, and on the other hand, it will absorb dust in the air and cause the polarizer to be contaminated. Therefore, it is very important to develop a pressure-sensitive adhesive with excellent adhesion, durability, and anti-static properties. In addition, most polarizer surfaces have been surface-treated and have different degrees of roughness. The pressure-sensitive adhesive used for the protective film must have excellent wettability and air-discharging properties for polarizers of different roughness in order to effectively protect the polarizer from contamination. The protective film must also have a low high-speed peeling force to facilitate the automated equipment to easily tear off the protective film during the panel manufacturing process.
[0004] Although the prior art provides relevant technical solutions, such as Chinese patent application CN113637436B discloses a pressure-sensitive adhesive for polarizer protective film, which is obtained by copolymerization of acrylic hard monomer, soft monomer, cross-linking monomer, amide-containing acrylic monomer, ether-containing acrylic monomer and vinyl silicone oil. Although the peeling force of this pressure-sensitive adhesive is 4 to 6 g / 50 mm (the industry's requirement for low-speed peeling force before aging: no more than 5 g / 25 mm), the solution does not provide the peeling force data after high-temperature aging and the high-speed peeling force data. For example, Chinese patent applications CN116694268A and CN106597596B proposed using N-methoxymethyl acrylamide or N-butoxymethyl acrylamide to improve the resistance of pressure-sensitive adhesive to wet heat aging, but these solutions did not provide high-speed peeling force data. How to provide an acrylic pressure-sensitive adhesive that meets the requirements of polarizer protective film in terms of adhesion, durability, antistatic properties, air discharge and high-speed peeling force is a problem that needs to be solved.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a high modulus acrylic pressure-sensitive adhesive and a preparation method thereof and a polarizer protective film, which have excellent adhesion, durability, antistatic properties, gas discharge and lower high-speed peeling force, thereby solving the above-mentioned technical problems existing in the prior art.
[0007] The objective of the present invention is achieved through the following technical solutions:
[0008] A high modulus acrylic pressure-sensitive adhesive, wherein the storage modulus of the acrylic pressure-sensitive adhesive after curing is 1 to 50×10 5 Pa, made from acrylate copolymer, antistatic agent, antioxidant, curing agent and diluent solvent as raw materials; wherein the side chain of the acrylate copolymer has alkyl, hydroxyl, carboxyl, amide, alkylamino, ethoxy and siloxane structures, and the weight average molecular weight of the acrylate copolymer is 500,000 to 1.5 million;
[0009] The acrylate copolymer is prepared by copolymerizing acrylate soft monomers, acrylate hard monomers, hydroxyl-containing acrylic monomers, carboxyl-containing acrylic monomers, acrylamide monomers, ethoxy-containing acrylic monomers and vinyl-terminated siloxane through solution free radical polymerization.
[0010] The solid content of the pressure-sensitive adhesive is 20% to 70%.
[0011] Preferably, in the above-mentioned pressure-sensitive adhesive, in the acrylic ester copolymer, the amounts of the hydroxyl-containing acrylic monomer, the carboxyl-containing acrylic monomer, the acrylamide monomer, the ethoxy-containing acrylic monomer, and the terminal vinyl siloxane are 1-10%, 0.1-10%, 1-50%, 1-50% and 0.01-10% of the total weight of the acrylic ester soft monomer and the acrylic ester hard monomer, respectively.
[0012] Preferably, in the above-mentioned pressure-sensitive adhesive, in the acrylic ester copolymer, the acrylic soft monomer is one or more of octadecyl acrylate, dodecyl acrylate, isooctyl acrylate, octyl acrylate, n-butyl acrylate, isobutyl acrylate, n-propyl acrylate, and ethyl acrylate;
[0013] The acrylic hard monomer is one or more of methyl acrylate, methyl methacrylate, acrylonitrile, styrene, isobutyl methacrylate, tert-butyl methacrylate, and vinyl acetate;
[0014] The hydroxyl-containing acrylic monomer is one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate;
[0015] The carboxyl-containing acrylic acid monomer is one or more of acrylic acid, methacrylic acid and itaconic acid;
[0016] The acrylamide monomer is one or more of N,N-dimethylaminopropyl acrylamide, N,N-dimethylaminopropyl methacrylamide, N,N-diethylaminopropyl acrylamide, N,N-diethylaminopropyl methacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, and acryloylmorpholine;
[0017] The ethoxy structure-containing acrylic acid monomer is one or more of ethoxyethoxyethyl acrylate, ethoxyethyl acrylate, ethoxyethoxymethyl acrylate, and 2-methoxyethyl acrylate;
[0018] The vinyl-terminated siloxane is one or more of vinyl-terminated polydimethylsiloxane, γ-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, and methylphenylvinyl silicone oil.
[0019] Preferably, in the above pressure-sensitive adhesive, the acrylate copolymer is prepared in the following manner, including:
[0020] Add acrylate soft monomer, acrylate hard monomer, hydroxyl-containing acrylic monomer, carboxyl-containing acrylic monomer, acrylamide monomer, ethoxy-containing acrylic monomer, vinyl-terminated siloxane, initiator and solvent into the reaction kettle and the drip tank respectively, mix well, 2 The temperature is raised under the atmosphere, and when the material refluxes and foams in the reactor, the material in the drip tank device is uniformly added, that is, the reaction is carried out by a two-stage solution free radical polymerization method, and the reaction temperature, titration time and the maximum value of the temperature in the reactor at the initial stage of titration are recorded, and then the external temperature is adjusted to 70-80°C. After the addition is completed, the first insulation reaction is carried out for 0.5-2 hours, and then the first initiator is added, and the second insulation reaction is carried out for 0.5-2 hours, and then the second initiator is added, and the third insulation reaction is carried out for 0.5-2 hours. After the third initiator is added, the insulation reaction is carried out for 3 hours, the temperature is lowered to below 40°C, a solvent is added to dilute, and the material is filtered and discharged after stirring to obtain the acrylic ester copolymer.
[0021] Preferably, in the above pressure-sensitive adhesive, the solvent is one or more of ethyl acetate, butanone, butyl acetate, methyl acetate, toluene, isopropanol, and methanol;
[0022] The initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, azobisisovaleronitrile, benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, and tert-amyl peroxy-2-ethylhexanoate.
[0023] Preferably, in the above-mentioned pressure-sensitive adhesive, the amount of the antistatic agent is 0.05 to 1% of the total weight of all monomers in the acrylic ester copolymer;
[0024] The amount of the antioxidant is 0.05-1% of the total weight of all monomers in the acrylic ester copolymer;
[0025] The amount of the curing agent used is 0.01-0.1% of the total weight of all monomers in the acrylic ester copolymer.
[0026] Preferably, in the above-mentioned pressure-sensitive adhesive, the antistatic agent is an ionic compound that is liquid or solid at room temperature; the antistatic agent is preferably at least one of an alkali metal inorganic salt and an alkali metal organic salt;
[0027] The antioxidant is one or more of aromatic amine antioxidants, hindered phenol antioxidants, phosphate antioxidants and thioether antioxidants;
[0028] The curing agent is one or more of trifunctional isocyanate, modified isocyanate compound and multifunctional epoxy compound.
[0029] A method for preparing the high modulus acrylic pressure-sensitive adhesive of the present invention comprises the following steps:
[0030] Take various raw materials according to the acrylate pressure-sensitive adhesive formula of the present invention;
[0031] An antistatic agent, an antioxidant, a curing agent and a diluent solvent are added to a pre-prepared acrylic copolymer having an alkyl, hydroxyl, carboxyl, amide, alkylamino, ethoxy and siloxane structure in the side chain, and the mixture is stirred evenly to obtain a high modulus acrylic pressure-sensitive adhesive.
[0032] Preferably, in the above method, an acrylate copolymer having a side chain having an alkyl group, a hydroxyl group, a carboxyl group, an amide group, an alkylamino group, an ethoxy group and a siloxane structure is prepared in advance in the following manner, including:
[0033] The raw materials are acrylic acid ester soft monomer, acrylic acid ester hard monomer, hydroxyl-containing acrylic acid monomer, carboxyl-containing acrylic acid monomer, acrylamide monomer, ethoxy-containing acrylic acid monomer, vinyl-terminated siloxane, initiator and solvent;
[0034] Add acrylate soft monomer, acrylate hard monomer, hydroxyl-containing acrylic monomer, carboxyl-containing acrylic monomer, acrylamide monomer, ethoxy-containing acrylic monomer, vinyl-terminated siloxane, initiator and solvent into the reaction kettle and the drip tank respectively, mix well, 2The temperature is raised under the atmosphere, and when the material in the reactor refluxes and foams, the material in the drip tank is uniformly added, that is, the reaction is carried out by a two-stage solution free radical polymerization method, and the reaction temperature, titration time and the maximum value of the temperature in the reactor at the initial stage of titration are recorded, and then the external temperature is adjusted to 70-80°C. After the addition is completed, the first insulation reaction is carried out for 0.5-2 hours, and then the first initiator is added, and the second insulation reaction is carried out for 0.5-2 hours, and then the second initiator is added, and the third insulation reaction is carried out for 0.5-2 hours. After the third initiator is added, the insulation reaction is carried out for 3 hours, the temperature is lowered to below 40°C, a solvent is added to dilute, and the material is filtered and discharged after stirring to obtain the acrylic ester copolymer.
[0035] A polarizer protective film is prepared by using the high modulus acrylate pressure-sensitive adhesive of the invention as a raw material through coating, drying, laminating and ripening in sequence.
[0036] Compared with the prior art, the high modulus acrylic pressure-sensitive adhesive and its preparation method and polarizer protective film provided by the present invention have the following beneficial effects:
[0037] By adding acrylamide monomers, ethoxy-containing acrylic monomers and terminal vinyl siloxane as special monomers to the acrylate copolymer, on the one hand, the acrylate copolymer is endowed with certain crystallization characteristics, and on the other hand, covalent bonds, hydrogen bonds and van der Waals forces are formed between the polymer molecules, thereby enhancing the cohesion and modulus of the polymer. It is also found that the side chain of this acrylate copolymer has hydroxyl, carboxyl, amide, alkylamino, ethoxy and siloxane structures. When N,N-dimethylacrylamide or N,N-diethylacrylamide and acrylamide are used as special monomers, the pressure-sensitive adhesive has excellent durability and low high-speed peeling force. Characterization by Fourier transform infrared spectroscopy (FT-IR) (such as Figure 1 The characteristic peaks of hydrogen bonding (<3500cm -1 ), which means that the carbonyl group in the acrylamide structural unit is easy to form hydrogen bonds with OH in the carboxyl group, hydroxyl (OH), and NH on the amide group. In addition, Figure 2 The X-ray diffraction (XRD) spectra of the product of the present invention and the conventional removable pressure-sensitive adhesive are shown. Compared with the conventional removable pressure-sensitive adhesive, the XRD characteristic peak of the product of the present invention shifts to a larger 2θ angle, indicating that the product of the present invention has a smaller intermolecular distance, indicating that its intermolecular force is stronger. Figure 3The transmission electron microscope (TEM) images of the product of the present invention and the conventional removable pressure-sensitive adhesive are shown. Under high magnification, only a crystalline region of about 3 nm is observed in the product of the present invention, indicating that a crystalline polymer exists in the product of the present invention. The above characterization method proves that the acrylate copolymer in the present invention can form a strong intermolecular interaction force by itself. The DMA test results show that the storage modulus of the cured pressure-sensitive adhesive in the present invention can reach 1 to 50×10 5 The above test results all verify the reasons why the pressure-sensitive adhesive in the present invention has excellent durability and relatively low high-speed peeling force. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0039] Figure 1 This is the FT-IR spectrum of the high modulus acrylic pressure-sensitive adhesive sample provided in the embodiment of the present invention.
[0040] Figure 2 XRD spectra of the high modulus acrylic pressure-sensitive adhesive sample provided in the embodiment of the present invention and the conventional removable pressure-sensitive adhesive as a control sample.
[0041] Figure 3 TEM images of high modulus acrylic pressure-sensitive adhesive samples provided by embodiments of the present invention and TEM images of conventional removable pressure-sensitive adhesives; wherein, images a and b are TEM images of the high modulus acrylic pressure-sensitive adhesive samples of the present invention at different magnifications, and images c and d are TEM images of conventional removable pressure-sensitive adhesives at different magnifications;
[0042] Figure 4 Schematic diagram of hydrogen bonding between molecules of acrylate copolymer in the high modulus acrylic pressure-sensitive adhesive provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0043] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0044] First, the terms that may be used in this article are explained as follows:
[0045] The term “and / or” means that either or both of them can be realized at the same time. For example, X and / or Y means both “X” or “Y” and “X and Y”.
[0046] The terms "include", "comprises", "contains", "has" or other descriptions with similar semantics should be interpreted as non-exclusive inclusion. For example, including certain technical feature elements (such as raw materials, components, ingredients, carriers, dosage forms, materials, dimensions, parts, components, mechanisms, devices, steps, procedures, methods, reaction conditions, processing conditions, parameters, algorithms, signals, data, products or products, etc.) should be interpreted as including not only certain technical feature elements explicitly listed, but also other technical feature elements known in the art that are not explicitly listed.
[0047] The term "consisting of..." means excluding any technical feature elements not explicitly listed. If this term is used in a claim, it will make the claim closed, so that it does not contain technical feature elements other than the technical feature elements explicitly listed, except for the conventional impurities related to them. If this term only appears in a clause of a claim, it only limits the elements explicitly listed in the clause, and the elements recorded in other clauses are not excluded from the overall claim.
[0048] The term "parts by mass" refers to the mass ratio relationship between multiple components. For example, if it is described that component X is x parts by mass and component Y is y parts by mass, then the mass ratio of component X to component Y is x:y. 1 part by mass can represent any mass, for example, 1 part by mass can be represented as 1 kg or 3.1415926 kg. The sum of the parts by mass of all components is not necessarily 100 parts, but can be greater than 100 parts, less than 100 parts or equal to 100 parts. Unless otherwise specified, the parts, proportions and percentages described herein are all measured by mass.
[0049] When concentration, temperature, pressure, size or other parameters are expressed in the form of a numerical range, the numerical range should be understood to specifically disclose all ranges formed by the pairing of any upper limit, lower limit, and preferred value in the numerical range, regardless of whether the range is explicitly stated; for example, if a numerical range of "2 to 8" is stated, the numerical range should be interpreted as including ranges such as "2 to 7", "2 to 6", "5 to 7", "3 to 4 and 6 to 7", "3 to 5 and 7", "2 and 5 to 7", etc. Unless otherwise specified, the numerical ranges stated herein include both their end values and all integers and fractions within the numerical range.
[0050] The scheme provided by the present invention is described in detail below. The contents not described in detail in the embodiments of the present invention belong to the prior art known to professionals in the field. If the specific conditions are not specified in the embodiments of the present invention, they are carried out according to the conventional conditions in the field or the conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used in the embodiments of the present invention, they are all conventional products that can be purchased commercially.
[0051] The embodiment of the present invention provides a high modulus acrylic pressure-sensitive adhesive, which is an acrylic pressure-sensitive adhesive for making a polarizer protective film, and has excellent adhesion, durability, antistatic properties, gas discharge and low high-speed peeling force. The pressure-sensitive adhesive is made of an acrylic ester copolymer, an antistatic agent, an antioxidant, a solvent and a curing agent, and the solid content of the pressure-sensitive adhesive is 20% to 70%, preferably 30% to 60%, wherein:
[0052] The side chain of the acrylic ester copolymer has an alkyl group, a hydroxyl group, a carboxyl group, an alkylamino group, an amide group, an ethoxy structure and a siloxane structure, and the weight average molecular weight of the acrylic ester copolymer is 500,000 to 1,000,000;
[0053] The structure of the acrylic acid ester copolymer having an alkyl group, a hydroxyl group, a carboxyl group, an amide group, an alkylamino group, an ethoxy structure and a siloxane structure in the side chain is shown in FIG. Figure 4 , Figure 4 The invention provides a schematic diagram of hydrogen bonding between molecules of acrylic ester copolymer. The acrylic ester copolymer is copolymerized by free radical polymerization of acrylic soft monomer, acrylic hard monomer, hydroxyl acrylic monomer, carboxyl acrylic monomer, acrylamide monomer, ethoxy structure acrylic monomer and vinyl-terminated siloxane through solution; wherein the hydroxyl acrylic monomer and carboxyl acrylic monomer are functional monomers; the acrylamide monomer, ethoxy structure acrylic monomer and vinyl-terminated siloxane are special monomers, and the amount of hydroxyl acrylic monomer, carboxyl acrylic monomer, acrylamide monomer, ethoxy structure acrylic monomer and vinyl-terminated siloxane is 1-10%, 0.1-10%, 1-50%, 1-50% and 0.01-10% of the total weight of the acrylic soft monomer and the acrylic hard monomer, respectively.
[0054] Preferably, in the above-mentioned acrylic ester copolymer, the acrylic soft monomer is one or more of octadecyl acrylate, dodecyl acrylate, isooctyl acrylate, n-butyl acrylate, isobutyl acrylate, n-propyl acrylate and ethyl acrylate.
[0055] The acrylic hard monomer is one or more of methyl acrylate, methyl methacrylate, acrylonitrile, styrene, isobutyl methacrylate, tert-butyl methacrylate and vinyl acetate.
[0056] The hydroxyl-containing acrylic monomer is one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate.
[0057] The carboxyl-containing acrylic acid monomer is one or more of acrylic acid, methacrylic acid and itaconic acid.
[0058] The acrylamide monomer is one or more of N,N-dimethylaminopropyl acrylamide, N,N-dimethylaminopropyl methacrylamide, N,N-diethylaminopropyl acrylamide, N,N-diethylaminopropyl methacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide and acryloylmorpholine.
[0059] The acrylic monomer containing an ethoxy structure is one or more of ethoxyethoxyethyl acrylate, ethoxyethyl acrylate, ethoxyethoxymethyl acrylate, and 2-methoxyethyl acrylate.
[0060] The vinyl-terminated siloxane includes one or more of vinyl-terminated polydimethylsiloxane, γ-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, and methylphenylvinyl silicone oil.
[0061] Preferably, in the pressure-sensitive adhesive, the acrylate copolymer is prepared in advance by solution free radical polymerization, comprising:
[0062] Add acrylic soft monomer, acrylic hard monomer, hydroxyl acrylic monomer, carboxyl acrylic monomer, acrylamide monomer, ethoxy acrylic monomer, vinyl-terminated siloxane, initiator and solvent into a reaction kettle (the reaction kettle is composed of a container, a four-mouth reaction kettle cover, a condenser, a thermometer, etc.) and a dropping tank device (the dropping tank device is composed of a beaker and a constant pressure dropping funnel) respectively and mix them evenly. The amount of initiator used in the reaction kettle and the dropping tank is 0.01% to 0.1% of the total weight of all monomers; the amount of solvent used in the reaction kettle and the dropping tank is 20% to 200% of the total weight of all monomers. 2 The reaction mixture was heated under a nitrogen atmosphere and heated to a temperature of 0.5 to 2 hours. When the material in the reactor refluxed and foamed, the material in the drip tank was uniformly added. The reaction was carried out by a two-stage solution free radical polymerization method. The reaction temperature, titration time and the maximum value of the internal temperature at the initial stage of titration were recorded. The external temperature was then adjusted to 70 to 80°C. After the addition was completed, the first insulation reaction was carried out for 0.5 to 2 hours. The first initiator was then added. The second insulation reaction was carried out for 0.5 to 2 hours. The second initiator was then added. The third insulation reaction was carried out for 0.5 to 2 hours. After the third initiator was added, the insulation reaction was carried out for 3 hours. The temperature was lowered to below 40°C, a solvent was added to dilute, the mixture was evenly stirred, and then filtered and discharged to obtain the acrylic ester copolymer.
[0063] In the above method, the role of recording the reaction temperature is: on the one hand, to confirm the temperature of the addition reaction of the primary free radical and the monomer; on the other hand, to compare with the production process parameters to ensure the correctness of the production operation.
[0064] The purpose of recording the titration time: take this moment as the starting point of the titration, derive the uniform dripping rate, and ensure that the material is dripped in a certain time.
[0065] Preferably, in the above-mentioned acrylic acid ester copolymer, the solvent is one or more of ethyl acetate, butanone, butyl acetate, methyl acetate, toluene, isopropanol and methanol;
[0066] The initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, azobisisovaleronitrile, benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, and tert-amyl peroxy-2-ethylhexanoate.
[0067] Preferably, in the pressure-sensitive adhesive, the amount of the antistatic agent is 0.05-1% of the total weight of all monomers in the acrylate copolymer. All monomers include acrylic soft monomers, acrylic hard monomers, functional monomers (i.e., hydroxyl-containing acrylic monomers, carboxyl-containing acrylic monomers) and special monomers (i.e., acrylamide monomers, ethoxy-containing acrylic monomers and vinyl-terminated siloxanes).
[0068] The amount of the antioxidant used is 0.05-1% of the total weight of all monomers in the acrylic ester copolymer.
[0069] The amount of the curing agent used is 0.01-0.1% of the total weight of all monomers in the acrylic ester copolymer.
[0070] Preferably, in the pressure-sensitive adhesive, the antistatic agent is an ionic compound that is liquid or solid at room temperature, and is preferably an inorganic salt of an alkali metal or an organic salt of an alkali metal.
[0071] Preferably, in the pressure-sensitive adhesive, the antioxidant is one or more of an aromatic amine antioxidant, a hindered phenol antioxidant, a phosphate antioxidant and a thioether antioxidant.
[0072] The curing agent is one or more of trifunctional isocyanate, modified isocyanate compound and multifunctional epoxy compound.
[0073] The present invention also provides a method for preparing the high modulus acrylic pressure-sensitive adhesive, comprising the following steps:
[0074] The raw materials are taken according to the above-mentioned acrylic pressure-sensitive adhesive formula; an antistatic agent, an antioxidant and a diluent solvent are added to the pre-prepared acrylic ester copolymer having an alkyl, hydroxyl, carboxyl, amide, alkylamino, ethoxy structure and siloxane structure in the side chain, and after stirring evenly, a curing agent is added and mixed evenly to obtain a high modulus acrylic pressure-sensitive adhesive.
[0075] Preferably, in the above method, an acrylic acid ester copolymer having an alkyl group, a hydroxyl group, a carboxyl group, an amide group, an alkylamino group, an ethoxy structure and a siloxane structure in the side chain is prepared in advance in the following manner, comprising: adding acrylic acid soft monomer, acrylic acid hard monomer, hydroxyl-containing acrylic acid monomer, carboxyl-containing acrylic acid monomer, acrylamide monomer, ethoxy-containing acrylic acid monomer, terminal vinyl siloxane, initiator and solvent into a reaction kettle and a drip tank device, respectively, and mixing them evenly; 2 The temperature is raised under the atmosphere, and when the materials in the reactor reflux and foam, the materials in the drip tank are uniformly added dropwise, and the reaction is carried out by two-stage solution free radical polymerization. The reaction temperature, titration time and the maximum value of the internal temperature at the initial stage of titration are recorded, and then the external temperature is adjusted to 70-80°C. After the addition is completed, the first heat preservation reaction is carried out for 0.5-2 hours, and then the first initiator is added, and the second heat preservation reaction is carried out for 0.5-2 hours, and then the second initiator is added, and the third heat preservation reaction is carried out for 0.5-2 hours. After the third initiator is added, the heat preservation reaction is carried out for 3 hours, and the temperature is lowered to below 40°C, and a solvent is added to dilute, and the acrylate copolymer is obtained after being evenly stirred and filtered. .
[0076] Furthermore, an embodiment of the present invention also provides a polarizer protective film, which is prepared by using the above-mentioned high modulus acrylic pressure-sensitive adhesive as a raw material through coating, drying, laminating, and aging in sequence.
[0077] In summary, the high modulus acrylic pressure-sensitive adhesive and the preparation method thereof according to the embodiment of the present invention have at least the following beneficial effects:
[0078] Introducing acrylamide monomers, ethoxy-containing acrylic monomers and terminal vinyl siloxane as special monomers into the acrylate copolymer not only endows the acrylate copolymer with certain crystallization characteristics, but also promotes the formation of covalent bonds, hydrogen bonds and van der Waals forces between polymers, see Figure 4 , thereby enhancing the cohesion and modulus of the polymer. It was also found that the side chain of this acrylate copolymer has hydroxyl, carboxyl, amide, alkylamino, ethoxy and siloxane structures. When N,N-dimethylacrylamide or N,N-diethylacrylamide and acrylamide are used as special monomers, the pressure-sensitive adhesive has excellent durability and low high-speed peeling force, as characterized by FT-IR (see Figure 1) observed the characteristic peak of associative hydrogen bonding, which means that the carbonyl group in the N,N-diethylacrylamide structural unit easily forms hydrogen bonds with OH in the carboxyl group, hydroxyl (OH), and NH on the amide group. In addition, Figure 2 The XRD spectra of the product of the present invention and a conventional removable pressure-sensitive adhesive are shown. Through XRD characterization, it is found that the characteristic peak of the product of the present invention shifts to a larger 2θ angle position, indicating that the product of the present invention has a smaller intermolecular distance, indicating that its intermolecular force is stronger. Figure 3 The TEM images of the product of the present invention and the conventional removable pressure-sensitive adhesive are shown. Through TEM characterization, it is found that under high magnification, only a crystalline region of about 3nm is observed in the product of the present invention, indicating that there are crystalline polymers in the product of the present invention. The above characterization method proves that the acrylate copolymer in the present invention can form a strong intermolecular interaction force. The DMA test results show that the storage modulus of the cured pressure-sensitive adhesive in the present invention can reach 1 to 50×10 5 Pa. The above structural test results all verify the reasons why the pressure-sensitive adhesive in the present invention has excellent durability and relatively low high-speed peeling force.
[0079] In order to more clearly demonstrate the technical solution and technical effects provided by the present invention, the high modulus acrylate pressure-sensitive adhesive and the preparation method thereof provided by the embodiments of the present invention are described in detail with reference to specific embodiments below.
[0080] Example 1
[0081] This embodiment provides a high modulus acrylic pressure-sensitive adhesive. The acrylic copolymer (X1) used in the acrylic pressure-sensitive adhesive has ingredients as shown in Table 1:
[0082] Table 1 Ingredients of Acrylate Copolymer X1
[0083]
[0084] The preparation method of the above-mentioned acrylic acid ester copolymer comprises the following steps:
[0085] Add the acrylic acid monomer, initiator and solvent listed in the table above into the reaction kettle and the dripping tank respectively, mix them evenly, and 2 In an atmosphere, the temperature is raised, and when the material in the reactor refluxes and foams, uniform dripping is started. After a period of dripping, the reaction is kept warm for a period of time, and then the initiator is added. The reaction is kept warm for a period of time, and then the initiator is added. After the initiator is added three times, the reaction is kept warm for 3 hours, the temperature is lowered to below 40°C, a solvent is added to dilute, and the material is discharged after stirring for a period of time to obtain an acrylate copolymer (X1).
[0086] The high modulus acrylate pressure-sensitive adhesive of this embodiment has ingredients as shown in Table 2:
[0087] Table 2 Ingredients of pressure-sensitive adhesive of Example 1
[0088]
[0089] The preparation method of the above-mentioned acrylic pressure-sensitive adhesive is as follows:
[0090] 0.2 g of antistatic agent, 0.2 g of antioxidant and diluent were added to 100 g of acrylate copolymer (X1), and after stirring evenly, 2.0 g of curing agent was added and stirred to obtain a high modulus acrylate pressure-sensitive adhesive.
[0091] Example 2
[0092] This embodiment provides a high modulus acrylic pressure-sensitive adhesive. Compared with the embodiment 1, the difference is that an acrylamide structure is added. The acrylic acid copolymer (X2) used in the acrylic pressure-sensitive adhesive has the following ingredient list:
[0093] Table 3 Ingredients of Acrylate Copolymer X2
[0094]
[0095] The preparation method of the acrylic acid ester copolymer (X2) of this example is the same as that of Example 1, please refer to Example 1.
[0096] The ingredient list and preparation method of the acrylic pressure-sensitive adhesive of this embodiment are the same as those of Embodiment 1, please refer to Embodiment 1.
[0097] Example 3
[0098] This embodiment provides a high modulus acrylic pressure-sensitive adhesive. Compared with Embodiment 1, the difference is that the weight proportion of the ethoxylated acrylic acid monomer is increased. The acrylic acid copolymer (X3) used in the acrylic pressure-sensitive adhesive has ingredients as shown in Table 4:
[0099] Table 4 Ingredients of Acrylate Copolymer X3
[0100]
[0101]
[0102] The preparation method of the acrylic acid ester copolymer (X3) of this example is the same as that of Example 1, please refer to Example 1.
[0103] The ingredient list and preparation method of the acrylic pressure-sensitive adhesive of this embodiment are the same as those of Embodiment 1, please refer to Embodiment 1.
[0104] Example 4
[0105] This embodiment provides a high modulus acrylic pressure-sensitive adhesive, which is different from Embodiment 2 in that a siloxane structure is added. The acrylic copolymer (X4) used in the acrylic pressure-sensitive adhesive has ingredients as shown in Table 5:
[0106] Table 5 Ingredients of Acrylate Copolymer X4
[0107]
[0108] The preparation method of the acrylic acid ester copolymer (X4) of this example is the same as that of Example 1, please refer to Example 1.
[0109] The ingredient list and preparation method of the acrylic pressure-sensitive adhesive of this embodiment are the same as those of Embodiment 1, please refer to Embodiment 1.
[0110] Comparative Example 1
[0111] This comparative example provides a high modulus acrylic pressure-sensitive adhesive. Compared with Example 1, no acrylamide monomer is added. The acrylic acid copolymer (D1) used in the acrylic pressure-sensitive adhesive has ingredients as shown in Table 6:
[0112] Table 6 Ingredients of Acrylate Copolymer D1
[0113]
[0114] The preparation method of the acrylic acid ester copolymer (D1) of this comparative example is the same as that of Example 1, please refer to Example 1.
[0115] The ingredient list and preparation method of the acrylic pressure-sensitive adhesive of this comparative example are the same as those of Example 1, please refer to Example 1.
[0116] Comparative Example 2
[0117] This comparative example provides a high modulus acrylic pressure-sensitive adhesive. Compared with Example 1, no ethoxylated acrylic acid monomer is added. The acrylic acid copolymer (D2) used in the acrylic pressure-sensitive adhesive has ingredients as shown in Table 7:
[0118] Table 7 Ingredients of Acrylate Copolymer D2
[0119]
[0120] The preparation method of the acrylic acid ester copolymer (D2) of this comparative example is the same as that of Example 1, please refer to Example 1.
[0121] The ingredient list and preparation method of the acrylic pressure-sensitive adhesive of this comparative example are the same as those of Example 1, please refer to Example 1.
[0122] Comparative Example 3
[0123] This comparative example provides a high modulus acrylic pressure-sensitive adhesive, which is different from Example 1 in that acrylic acid, acrylamide monomers and ethoxylated acrylic acid monomers are not added. The acrylic acid copolymer (D3) used in the acrylic pressure-sensitive adhesive has ingredients as shown in Table 8:
[0124] Table 8 Ingredients of Acrylate Copolymer D3
[0125]
[0126] The preparation method of the acrylic acid ester copolymer (D3) of this comparative example is the same as that of Example 1, please refer to Example 1.
[0127] The ingredient list and preparation method of the acrylic pressure-sensitive adhesive of this comparative example are the same as those of Example 1, please refer to Example 1.
[0128] It can be known that the above comparative examples 1, 2 and 3 are specially designed for comparing the performance of the product of the present invention, and they are not prior arts.
[0129] The polarizer protective films were prepared by coating, drying, laminating and aging according to Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, respectively, and the following tests were performed:
[0130] 180° peel strength test: Determined in accordance with GB / T 2792-2014. The prepared tape (90×25mm) was pasted on a mirror steel plate, rolled back and forth once with a 2kg roller, and placed in a 23℃-50%RH environment for 20min or 24hr, and then the peel strength was measured by a tensile tester at a test speed of 300mm / min or 30m / min.
[0131] Adhesive layer resistance test: Cut the protective film into A4 size, tear off the release film, and test the adhesive surface resistance on a high resistance meter.
[0132] Durability test: The prepared tape (90×25mm) was pasted on the polarizer and rolled back and forth once with a 2kg roller. The sample was placed in an oven at 80°C for 7 days, 1 month, and 3 months, and the peeling force was measured by a tensile tester. The test speed was 300mm / min or 30m / min.
[0133] Residual adhesive resistance test: The prepared tape (90×25mm) was pasted on the polarizer and rolled back and forth once with a 2kg roller. The sample was placed in an oven at 85°C for 1 day, 3 days, and 7 days, and then the polarizer was observed for residual adhesive.
[0134] The test results for a medium haze polarizer are shown in Table 9.
[0135] Table 9 Test data of high modulus acrylic pressure-sensitive adhesive
[0136]
[0137] It can be seen from Table 9 that the pressure-sensitive adhesive product of the present invention has low high-speed peeling force, excellent durability, wettability and stable antistatic properties, and can well meet the requirements of polarizer protective film.
[0138] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.
Claims
1. A high modulus acrylic pressure-sensitive adhesive, characterized in that: The storage modulus of the acrylic pressure-sensitive adhesive at 100 Hz after curing is 1 to 50 × 10 5 Pa, made from acrylate copolymer, antistatic agent, antioxidant, curing agent and solvent as raw materials; wherein the side chain of the acrylate copolymer has alkyl, hydroxyl, carboxyl, amide, alkylamino, ethoxy and siloxane structures, and the weight average molecular weight of the acrylate copolymer is 500,000 to 1.5 million; The acrylate copolymer is prepared by copolymerizing acrylate soft monomers, acrylate hard monomers, hydroxyl-containing acrylic monomers, carboxyl-containing acrylic monomers, acrylamide monomers, ethoxy-containing acrylic monomers and vinyl-terminated siloxane through solution free radical polymerization. The solid content of the pressure-sensitive adhesive is 20% to 70%.
2. The high modulus acrylic pressure-sensitive adhesive according to claim 1, characterized in that: In the acrylic ester copolymer, the amounts of the hydroxyl-containing acrylic monomer, carboxyl-containing acrylic monomer, acrylamide monomer, ethoxy-containing acrylic monomer and terminal vinyl siloxane are 1-10%, 0.1-10%, 1-50%, 1-50% and 0.01-10% of the total weight of the acrylic ester soft monomer and the acrylic ester hard monomer, respectively.
3. The high modulus acrylic pressure-sensitive adhesive according to claim 1, characterized in that: In the acrylic ester copolymer, the acrylic soft monomer is one or more of octadecyl acrylate, dodecyl acrylate, isooctyl acrylate, octyl acrylate, n-butyl acrylate, isobutyl acrylate, n-propyl acrylate, and ethyl acrylate; The acrylic hard monomer is one or more of methyl acrylate, methyl methacrylate, acrylonitrile, styrene, isobutyl methacrylate, tert-butyl methacrylate, and vinyl acetate; The hydroxyl-containing acrylic monomer is one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate; The carboxyl-containing acrylic acid monomer is one or more of acrylic acid, methacrylic acid and itaconic acid; The acrylamide monomer is one or more of N,N-dimethylaminopropyl acrylamide, N,N-dimethylaminopropyl methacrylamide, N,N-diethylaminopropyl acrylamide, N,N-diethylaminopropyl methacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, and acryloylmorpholine; The ethoxy structure-containing acrylic acid monomer is one or more of ethoxyethoxyethyl acrylate, ethoxyethyl acrylate, ethoxyethoxymethyl acrylate, and 2-methoxyethyl acrylate; The vinyl-terminated siloxane is one or more of vinyl-terminated polydimethylsiloxane, γ-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, and methylphenylvinyl silicone oil.
4. The high modulus acrylic pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The acrylic acid ester copolymer is prepared in the following manner, comprising: Add acrylate soft monomer, acrylate hard monomer, hydroxyl acrylic monomer, carboxyl acrylic monomer, acrylamide monomer, ethoxy structure acrylic monomer, terminal vinyl siloxane, initiator and solvent into the reaction kettle and mix them evenly. Heat and raise the temperature under N2 atmosphere. When the material refluxes and foams in the reaction kettle, start to drop the material in the dropping tank at a uniform speed, that is, adopt a two-stage solution free radical polymerization method to react. Record the reaction temperature, titration time and the maximum value of the temperature in the reaction kettle at the initial titration stage, then adjust the external temperature to 70-80°C. After the dropwise addition is completed, carry out the first heat preservation reaction for 0.5-2 hours, then add the first initiator, carry out the second heat preservation reaction for 0.5-2 hours, then add the second initiator, carry out the third heat preservation reaction for 0.5-2 hours, then add the third initiator, carry out the third heat preservation reaction for 3 hours, cool to below 40°C, add solvent to dilute, stir evenly, filter and discharge to obtain the acrylate copolymer.
5. The high modulus acrylic pressure-sensitive adhesive according to claim 4, characterized in that: The solvent is one or more of ethyl acetate, butanone, butyl acetate, methyl acetate, toluene, isopropanol, and methanol; The initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, azobisisovaleronitrile, benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, and tert-amyl peroxy-2-ethylhexanoate.
6. The high modulus acrylate pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The amount of the antistatic agent is 0.05-1% by weight of the total acrylate monomer; The antioxidant is used in an amount of 0.05 to 1% by weight of all acrylate monomers in the acrylate copolymer; The amount of the curing agent used is 0.01-0.1% of the total weight of all acrylate monomers in the acrylate copolymer.
7. The high modulus acrylate pressure-sensitive adhesive according to any one of claims 1 to 3, characterized in that: The antistatic agent is an ionic compound that is liquid or solid at room temperature; The antioxidant is one or more of aromatic amine antioxidants, hindered phenol antioxidants, phosphate antioxidants and thioether antioxidants; The curing agent is one or more of trifunctional isocyanate, modified isocyanate compound and multifunctional epoxy compound.
8. A method for preparing the high modulus acrylic pressure-sensitive adhesive according to any one of claims 1 to 7, characterized in that: The following steps are involved: Take the raw materials according to the acrylate pressure-sensitive adhesive formula according to any one of claims 1 to 7; An antistatic agent, an antioxidant, a curing agent and a solvent are added to a pre-prepared acrylic copolymer having an alkyl, hydroxyl, carboxyl, amide, alkylamino, ethoxy and siloxane structure in the side chain, and the mixture is stirred evenly to obtain a high modulus acrylic pressure-sensitive adhesive.
9. The method for preparing a high modulus acrylic pressure-sensitive adhesive according to claim 8, characterized in that: An acrylate copolymer having an alkyl, hydroxyl, carboxyl, amide, alkylamino, ethoxy and siloxane structure in the side chain is prepared in advance in the following manner, including: The raw materials are acrylic acid ester soft monomer, acrylic acid ester hard monomer, hydroxyl-containing acrylic acid monomer, carboxyl-containing acrylic acid monomer, acrylamide monomer, ethoxy-containing acrylic acid monomer, vinyl-terminated siloxane, initiator and solvent; Add acrylate soft monomer, acrylate hard monomer, hydroxyl acrylic monomer, carboxyl acrylic monomer, acrylamide monomer, ethoxy structure acrylic monomer, terminal vinyl siloxane, initiator and solvent into the reaction kettle and drip tank device respectively, mix them evenly, heat and raise the temperature under N2 atmosphere, and when the material in the reaction kettle refluxes and foams, start to uniformly drip the material in the drip tank, that is, adopt a two-stage solution free radical polymerization method to react, record the reaction temperature, titration time and the maximum value of the temperature in the reaction kettle at the initial titration stage, then adjust the external temperature to 70-80°C, after the dripping is completed, carry out the first insulation reaction for 0.5-2 hours, then add the first initiator, carry out the second insulation reaction for 0.5-2 hours, then add the second initiator, carry out the third insulation reaction for 0.5-2 hours, add the third initiator, carry out the insulation reaction for 3 hours, cool to below 40°C, add solvent to dilute, stir evenly, filter and discharge to obtain the acrylate copolymer.
10. A polarizer protective film, characterized in that: The polarizer protective film is prepared by using the high modulus acrylic pressure-sensitive adhesive described in any one of claims 1 to 7 as a raw material through coating, drying, laminating and aging in sequence.
Citation Information
Patent Citations
A pressure-sensitive adhesive for polarizer protective film and the polarizer protective film thereof.
CN106597596B
An acrylic pressure-sensitive adhesive, its preparation method, and a polarizer protective film.
CN113637436B
Pressure-sensitive adhesive for polaroid as well as preparation method and application of pressure-sensitive adhesive
CN116694268A
Cited By
Novel polyacrylate pressure-sensitive adhesive for protective film and preparation method of novel polyacrylate pressure-sensitive adhesive
CN121022313A