Underfill adhesive with low curing shrinkage rate and preparation method thereof
By using expanded monomers and other components with specific proportions in the underfill glue, the problem of high curing shrinkage of traditional underfill glue is solved, low curing shrinkage and high adhesion are achieved, and the reliability of the packaging material is improved. and glue fluidity.
Patent Information
- Application Number
- CN202411196767.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional underfill glues produce higher curing shrinkage during the curing process, resulting in unstable and reliability problems in the packaging composite material. The existing methods reduce shrinkage by adding a large amount of filler but affect the fluidity of the glue.
The bottom with low curing shrinkage is prepared by synthesizing the expanded monomer and mixing it under low temperature vacuum conditions using epoxy resins, toughening agents, curing agents, cationic initiators, carbon black and fillers with specific ratios. Fill glue.
It effectively reduces the curing shrinkage rate, reduces the curing shrinkage stress, improves the reliability of the packaging material, and maintains the fluidity of the glue, avoiding the negative impact of filler addition on viscosity.
Smart Images

Figure BDA0005016664470000021 
Figure BDA0005016664470000071 
Figure FDA0005016664460000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a bottom filling adhesive with low curing shrinkage and a preparation method thereof. Background Art
[0002] With the development of the electronics industry and the changes in market demand, chip design is developing towards functionalization, high speed, low energy consumption and miniaturization, and the requirements for chip integration are getting higher and higher. In order to meet these requirements, the requirements for chip packaging technology are also getting higher and higher, and the packaging process has also been continuously developed. Traditional packaging includes all technical contents from zero-level packaging to three-level packaging, among which the mutual or sealed connection between chips is called first-level packaging, which mainly includes wire bonding, flip-chip welding, automatic tape welding and silicon through-holes. Due to the different coefficients of thermal expansion (CTE) between the chip and the substrate, reliability problems will occur during use, causing significant losses, so bottom filling technology came into being. The bottom filling glue technology uses the capillary action of the bottom filling glue to fill the gap between the chip and the substrate, and is used to be placed under the chip to fill the gap between the chip and the substrate. The cured bottom filling glue has a high modulus, a coefficient of thermal expansion (CTE) that matches the solder joint, and has good adhesion. It can redistribute the stress of the substrate, chip, solder ball and bottom filling glue, ensuring the reliability of the chip in the subsequent use process.
[0003] Traditional bottom filler is mainly composed of epoxy resin, curing agent, silicon dioxide and auxiliary agent. During the curing process, epoxy resin and curing agent are monomer molecules that exist in the interaction of van der Waals force at the beginning. As the curing reaction proceeds, the monomer molecules are connected by covalent bonds, and the distance between molecules disappears, resulting in volume shrinkage during the curing process, which makes the packaging composite material cracked and dimensional unstable. In addition, after the resin reaches the gel point, the mobility of the molecular chain network decreases, forming a part of the curing shrinkage stress. And when the packaging composite material is cured, due to the shrinkage of the glass state, a part of the shrinkage stress will be generated. These residual stresses will cause the packaging device to warp, crack and other phenomena, and will still affect the reliability of the packaging material. Therefore, it is of great significance to improve the curing shrinkage rate of the bottom filler, reduce the residual stress caused by it, and thus improve the reliability of the packaging material.
[0004] Current bottom filling adhesive products reduce the curing shrinkage by adding a large amount of fillers, which will increase the viscosity of the adhesive, affecting its fluidity during use and the effect of the bottom filling. Summary of the invention
[0005] In view of the above deficiencies in the prior art, an object of the present invention is to provide a bottom filling glue with low curing shrinkage and a preparation method thereof, which does not require adding a large amount of fillers and sacrificing the fluidity of the glue to reduce the curing shrinkage.
[0006] To achieve the above objectives, the technical solutions adopted are:
[0007] One of the purposes of the present invention is to provide a bottom filling glue with low curing shrinkage, which comprises the following components by weight: 50 to 80 parts of epoxy resin, 5 to 25 parts of expansion monomer, 4 to 10 parts of toughening agent, 8 to 15 parts of curing agent, 0.5 to 3 parts of cationic initiator, 0.1 to 0.5 parts of carbon black, and 10 to 30 parts of filler.
[0008] Preferably, the synthesis of the expandable monomer comprises the following steps: 1) mixing 7-30 g of diol with 20 g-30 g of di-n-butyltin oxide, and adding 300-500 ml of toluene to dissolve, then heating to 105-115° C. and reflux for 12 hours, and removing the water generated in the reaction with a water separator; 2) slowly adding 8-12 ml of carbon disulfide, and continuing to reflux at 105-115° C. for 12 hours; 3) removing the solvent toluene by reduced pressure distillation to obtain the product expandable monomer.
[0009] More preferably, the synthetic reaction formula of the expansion monomer is:
[0010]
[0011] The R group is at least one of a hydrogen atom, a methyl group, a p-methoxybenzylidene group, or other groups required according to performance.
[0012] Preferably, the epoxy resin is a mixture of one or more of bisphenol F epoxy resin, novolac epoxy resin, naphthalene epoxy resin, and biphenyl epoxy resin. More preferably, the bisphenol F epoxy resin is EPICLON 830 or 835 of DIC of Japan; the novolac epoxy resin is Dow DEN 438, Huntsman ARALDITE ECN 1273 or 1280; the naphthalene epoxy resin is SE-165 or SE-200 of SHIN-A of South Korea; and the biphenyl epoxy resin is TT4000 or YX4000 of Mitsubishi of Japan.
[0013] Preferably, the toughening agent is a core-shell rubber modified epoxy resin toughening agent, and more preferably, the toughening agent is MX125, MX153 or MX167 produced by Japan KANEKA.
[0014] Preferably, the curing agent is a tertiary amine adduct. More preferably, the tertiary amine adduct is MY-H, MY-24 or MY-25 from AJICURE of Japan.
[0015] Preferably, the cationic initiator is a mixture of one or more of a blocked Lewis acid salt, a blocked phosphate, and a blocked iodate. More preferably, the blocked Lewis acid salt is one or a combination of two of boron trifluoride monoethylamine (BF3·MEA) and boron trifluoride diethylamine (BF3·OEt2).
[0016] Preferably, the filler is spherical silica.
[0017] A second object of the present invention is to provide a method for preparing the above-mentioned bottom filling glue with low curing shrinkage, comprising the following steps:
[0018] (1) Weigh 50-80 parts of epoxy resin, 5-25 parts of expansion monomer, and 4-10 parts of toughening agent, put them into a high-speed planetary mixer and stir for 1-2 hours to mix them evenly; (2) Weigh 0.5-3 parts of cationic initiator, 8-15 parts of curing agent, 0.1-0.5 parts of carbon black, and 10-30 parts of filler, put them into a high-speed planetary mixer, control the temperature below 30°C, stir for 1-2 hours under vacuum, and mix them evenly to obtain a filling glue.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The bottom filling glue prepared by the present invention has the characteristics of low curing shrinkage, high adhesion, low viscosity, etc. Under the action of the expansion monomer, the curing shrinkage is effectively reduced, the curing shrinkage stress is reduced, and the reliability of the packaged components is guaranteed; and because it is not necessary to reduce the curing shrinkage by adding a high proportion of fillers, the viscosity of the system is greatly reduced, the fluidity of the glue is improved, and the use requirements of chip packaging are well met. DETAILED DESCRIPTION
[0021] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0022] Embodiment 1:
[0023] A method for preparing an underfill adhesive with low curing shrinkage comprises the following steps:
[0024] (1) Preparation of expansion monomer:
[0025] 1) 8g of 1,3-propylene glycol and 25g of di-n-butyltin oxide were added into a three-necked flask, and 300ml of toluene was added to dissolve, and then heated to 108°C and refluxed for 12h, and the water generated in the reaction was removed with a water separator; 2) 8ml of carbon disulfide was slowly added dropwise, and the temperature was kept at 108°C and refluxed for 12h; 3) the solvent toluene was removed by reduced pressure distillation to obtain the product expansion monomer.
[0026] (2) Preparation of bottom filler
[0027] Weigh 60g of EPICLON 830 epoxy resin, 20g of ARALDITE ECN 1273 epoxy resin, 10g of expansion monomer, and 10g of KANEKA toughening agent MX125, put them into a high-speed planetary stirrer and stir for 1h at a speed of 300r / min to mix evenly; weigh 3g of cationic initiator boron trifluoride monoethylamine, 10g of curing agent MY-H, 0.2g of carbon black, and 20g of filler spherical silica, put them into a high-speed planetary stirrer, control the temperature below 30°C, maintain the vacuum degree not lower than -0.08Mpa, stir at a speed of 300r / min for 1h, mix evenly, and obtain the filling glue.
[0028] Embodiment 2:
[0029] A method for preparing an underfill adhesive with low curing shrinkage comprises the following steps:
[0030] (1) Preparation of expansion monomer:
[0031] 1) Add 9g of 2-methyl-1,3-propanediol and 25g of di-n-butyltin oxide into a three-necked flask, and add 300ml of toluene to dissolve, then heat to 108°C and reflux for 12h, and use a water separator to remove the water generated in the reaction; 2) slowly add 8ml of carbon disulfide, and continue to reflux at 108°C for 12h; 3) remove the solvent toluene by reduced pressure distillation to obtain the product expansion monomer.
[0032] (2) Preparation of bottom filler
[0033] Weigh 60g of EPICLON 830 epoxy resin, 20g of ARALDITE ECN 1273 epoxy resin, 10g of expansion monomer, and 10g of KANEKA toughening agent MX125, put them into a high-speed planetary stirrer and stir for 1h at a speed of 300r / min to mix evenly; weigh 3g of cationic initiator boron trifluoride monoethylamine, 10g of curing agent MY-H, 0.2g of carbon black, and 20g of filler spherical silica, put them into a high-speed planetary stirrer, control the temperature below 30°C, maintain the vacuum degree not lower than -0.08Mpa, stir at a speed of 300r / min for 1h, mix evenly, and obtain the filling glue.
[0034] Embodiment 3:
[0035] A method for preparing an underfill adhesive with low curing shrinkage comprises the following steps:
[0036] (1) Preparation of expansion monomer:
[0037] Same as Example 2.
[0038] (2) Preparation of bottom filler
[0039] Weigh 60g of EPICLON 830 epoxy resin, 20g of ARALDITE ECN 1273 epoxy resin, 15g of expansion monomer, and 10g of KANEKA toughening agent MX125, put them into a high-speed planetary stirrer and stir for 1h at a speed of 300r / min to mix evenly; weigh 3g of cationic initiator boron trifluoride monoethylamine, 10g of curing agent MY-H, 0.2g of carbon black, and 20g of filler spherical silica, put them into a high-speed planetary stirrer, control the temperature below 30°C, maintain the vacuum degree not lower than -0.08Mpa, stir at a speed of 300r / min for 1h, mix evenly, and obtain the filling glue.
[0040] Embodiment 4:
[0041] A method for preparing an underfill adhesive with low curing shrinkage comprises the following steps:
[0042] (1) Preparation of expansion monomer:
[0043] Same as Example 2.
[0044] (2) Preparation of bottom filler
[0045] Weigh 60g of EPICLON 830 epoxy resin, 20g of ARALDITE ECN 1273 epoxy resin, 20g of expansion monomer, and 10g of KANEKA toughening agent MX125, put them into a high-speed planetary stirrer and stir for 1h at a speed of 300r / min to mix evenly; weigh 3g of cationic initiator boron trifluoride monoethylamine, 10g of curing agent MY-H, 0.2g of carbon black, and 20g of filler spherical silica, put them into a high-speed planetary stirrer, control the temperature below 30°C, maintain the vacuum degree not lower than -0.08Mpa, stir at a speed of 300r / min for 1h, mix evenly, and obtain the filling glue.
[0046] Comparative Example 1:
[0047] A method for preparing an underfill adhesive with low curing shrinkage comprises the following steps:
[0048] Weigh 60g of EPICLON 830 epoxy resin, 20g of ARALDITE ECN 1273 epoxy resin, and 10g of KANEKA toughening agent MX125, put them into a high-speed planetary stirrer and stir for 1h at a speed of 300r / min to mix evenly; weigh 3g of cationic initiator boron trifluoride monoethylamine, 10g of curing agent MY-H, 0.2g of carbon black, and 20g of filler spherical silica, put them into a high-speed planetary stirrer, control the temperature below 30°C, maintain the vacuum degree not lower than -0.08Mpa, stir at a speed of 300r / min for 1h, mix evenly, and obtain the filling glue.
[0049] Comparative Example 2:
[0050] A method for preparing an underfill adhesive with low curing shrinkage comprises the following steps:
[0051] Weigh 60g of EPICLON 830 epoxy resin, 20g of ARALDITE ECN 1273 epoxy resin, and 10g of KANEKA toughening agent MX125, put them into a high-speed planetary stirrer and stir for 1h at a speed of 300r / min to mix evenly; weigh 3g of cationic initiator boron trifluoride monoethylamine, 10g of curing agent MY-H, 0.2g of carbon black, and 60g of filler spherical silica, put them into a high-speed planetary stirrer, control the temperature below 30°C, maintain the vacuum degree not lower than -0.08Mpa, stir at a speed of 300r / min for 1h, mix evenly, and obtain the filling glue.
[0052] test
[0053] The curing shrinkage rate of Examples 1 to 4 and Comparative Examples 1 to 2 was tested according to the standard GB / T 24148.9-2014 after curing at 150°C for 30 minutes. The viscosity was tested using a HAAKE rotary viscometer (test conditions: 25°C, C35 / 2, 20s -1 ), the test data is shown in the following table:
[0054] Table 1. Performance test data of Examples 1 to 4 and Comparative Examples 1 to 2
[0055]
[0056] Through comparative tests, it was found that the effect of reducing the curing shrinkage rate of the expansion monomer structure in Example 2 is better than that of the expansion monomer in Example 1. This is because the polymerization activity of the expansion monomer structure in Example 2 is closer to the epoxy system. According to the polymerization activity of epoxy resins with different structures, expansion monomers with different structures can be selected; in Examples 2 to 4, as the content of the expansion monomer increases, the curing shrinkage rate also decreases. In addition, the use of expansion monomers can effectively dilute the viscosity of the system. Comparative Example 1 does not use expansion monomers, its viscosity is higher, and the curing shrinkage rate is higher; Comparative Example 2 increases the filler content, and the curing shrinkage rate is reduced to a certain extent, but the viscosity is also higher, which is not conducive to the flow of glue.
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A bottom filling adhesive with low curing shrinkage, characterized in that: The composition comprises the following components by weight: 50-80 parts of epoxy resin, 5-25 parts of expansion monomer, 4-10 parts of toughening agent, 8-15 parts of curing agent, 0.5-3 parts of cationic initiator, 0.1-0.5 parts of carbon black and 10-30 parts of filler.
2. The bottom filling adhesive with low curing shrinkage according to claim 1, characterized in that: The synthesis of the expandable monomer comprises the following steps: 1) mixing 7-30g of diol with 20g-30g of di-n-butyltin oxide, and adding 300-500ml of toluene to dissolve, then heating to 105-115°C and refluxing for 12h, and removing water generated in the reaction with a water separator; 2) slowly adding 8-12ml of carbon disulfide, and continuing to reflux at 105-115°C for 12h; 3) removing the solvent toluene by reduced pressure distillation to obtain the product expandable monomer.
3. The bottom filling adhesive with low curing shrinkage according to claim 1, characterized in that: The synthetic reaction formula of the expansion monomer is: The R group is at least one of a hydrogen atom, a methyl group, and a p-methoxybenzylidene group.
4. The bottom filling adhesive with low curing shrinkage according to claim 1, characterized in that: The epoxy resin is a mixture of one or more of bisphenol F epoxy resin, phenolic epoxy resin, naphthalene epoxy resin and biphenyl epoxy resin.
5. The bottom filling adhesive with low curing shrinkage according to claim 1, characterized in that: The toughening agent is a core-shell rubber modified epoxy resin toughening agent.
6. The bottom filling adhesive with low curing shrinkage according to claim 1, characterized in that: The curing agent is a tertiary amine adduct.
7. The bottom filling adhesive with low curing shrinkage according to claim 1, characterized in that: The cationic initiator is a mixture of one or more of blocked Lewis acid salts, blocked phosphates and blocked iodates.
8. The bottom filling adhesive with low curing shrinkage according to claim 1, characterized in that: The filler is spherical silica.
9. A method for preparing an underfill adhesive with low curing shrinkage as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Weigh 50-80 parts of epoxy resin, 5-25 parts of expansion monomer, and 4-10 parts of toughening agent, put them into a high-speed planetary mixer and stir for 1-2 hours to mix them evenly; (2) Control the temperature below 30°C, weigh 0.5-3 parts of cationic initiator, 8-15 parts of curing agent, 0.1-0.5 parts of carbon black, and 10-30 parts of filler, put them into a high-speed planetary mixer, stir for 1-2 hours under vacuum, and mix them evenly to obtain a filling glue.