Flame-retardant organic silicon bi-component heat-conducting pouring sealant and preparation method thereof

By modifying vermiculite with silane coupling agent, sodium ion and ion flame retardant liquid, a flame retardant silicone two-component thermal potting adhesive is solved, and the thermal conductivity reduction caused by the addition of flame retardant in the prior art is solved and The smoke generation problem has achieved a balance between high thermal conductivity and good flame retardant effects.

CN119039934AInactive Publication Date: 2024-11-29佛山禾邦新材料科技有限公司

Patent Information

Application Number
CN202411381404.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When the existing silicone thermal potting glue is added with flame retardant, the thermal conductivity of the existing silicone thermal potting glue will decrease and produce a large amount of smoke, affecting the environment and the safety of electronic components.

Method used

Modified vermiculite is modified by silane coupling agent, sodium ion and ionic flame retardant liquid to form a flame retardant silicone two-component thermal potting adhesive, which improves the limit oxygen index and flame retardant performance, and reduces the addition of flame retardant quantity.

Benefits of technology

While maintaining high thermal conductivity, the flame retardant performance is significantly improved, the use of flame retardant is reduced, the generation of smoke is avoided, and the safety and environmental friendliness of electronic components are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

In order to solve the problems that heat-conducting filler is reduced due to the fact that more flame retardants are added into an existing organic silicon heat-conducting pouring sealant, and the heat-conducting property is influenced, the invention provides a flame-retardant organic silicon two-component heat-conducting pouring sealant and a preparation method thereof, and the organic silicon two-component heat-conducting pouring sealant comprises a component A and a component B in parts by weight, the component A is prepared from 40 to 60 parts of double-end vinyl silicone oil, 16 to 25 parts of modified vermiculite, 120 to 180 parts of heat-conducting filler and 0.1 to 0.5 part of catalyst; the component B comprises the following components in parts by weight: 21-50 parts of hydrogen-containing silicone oil, 30-50 parts of double-end vinyl silicone oil, 16-25 parts of modified vermiculite and 120-180 parts of heat-conducting filler; the modified vermiculite is sequentially subjected to silane coupling agent graft modification, sodium ion modification and ionic flame-retardant liquid modification. According to the flame-retardant organic silicon bi-component heat-conducting pouring sealant provided by the invention, only 3-6% of modified vermiculite is added, a relatively good flame-retardant effect can be achieved by adding a small amount of modified vermiculite, the heat-conducting property of the organic silicon bi-component heat-conducting pouring sealant is not influenced, and the organic silicon bi-component heat-conducting pouring sealant is high in heat-conducting property, good in flame-retardant effect and free of sedimentation problem.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermally conductive potting adhesives, and in particular to a flame retardant organic silicon two-component thermally conductive potting adhesive and a preparation method thereof. Background Art

[0002] With the increasing development of the electronic and electrical industry, electronic products are developing towards high integration, high power and small miniaturization to meet the needs of emerging markets. However, high integration, high power and small miniaturization will cause a sharp increase in the heat generated per unit area of ​​electronic components. If it cannot be conducted out in time, the performance and life of electronic and electrical products will be seriously affected. At the same time, the scope of application of electronic and electrical products is becoming wider and wider. In many cases, the conditions in the application field are harsh, such as alternating high and low temperatures, high pressure, high-speed rotation, etc., which requires the potting material to have good flame retardancy to ensure the safety of product use. At present, most of the commonly used potting materials are high molecular polymers, which generally have the same disadvantages, that is, poor thermal conductivity and easy to burn. Therefore, it is of great significance to develop and research potting materials with both thermal conductivity and flame retardancy.

[0003] To address the above problems, a commonly used method in this field is to use a thermally conductive potting compound with thermal conductivity and flame retardant properties. The thermally conductive potting compound can effectively transfer the heat generated by electronic components during use to the housing, while also playing a role in fixing, waterproofing, dustproofing and shockproofing.

[0004] In order to meet the flame retardant properties of existing silicone thermal potting adhesives, more flame retardants must be added, such as aluminum hydroxide, IPPP, APP, etc. However, when these flame retardants are introduced into the system, the amount of thermal conductive filler will be reduced, which will affect the thermal conductivity. At the same time, most of the organic combustion aids added contain halogens, which are highly corrosive to electronic components. In addition, a large amount of smoke will be generated during the flame retardant experiment, causing serious impact on the environment.

[0005] Therefore, a filler is needed that can achieve a flame retardant effect when added in a relatively small amount, and can meet the thermal conductivity and flame retardant properties of silicone thermal conductive potting glue. Summary of the invention

[0006] In order to solve the problem that the existing organic silicon thermal conductive potting adhesive adds more flame retardants, resulting in a reduction in thermal conductive fillers and affecting thermal conductivity, the present application provides a flame retardant organic silicon two-component thermal conductive potting adhesive and a preparation method thereof.

[0007] On the one hand, the present application provides a flame retardant organic silicon two-component thermally conductive potting adhesive, comprising component A and component B, in parts by weight: The component A comprises 40-60 parts of double-terminal vinyl silicone oil, 16-25 parts of modified vermiculite, 120-180 parts of thermal conductive filler, and 0.1-0.5 parts of catalyst; The B component includes 21 to 50 parts of hydrogenated silicone oil, 30 to 50 parts of double-terminal vinyl silicone oil, 16 to 25 parts of modified vermiculite, and 120 to 180 parts of thermal conductive filler; The modified vermiculite is obtained by sequentially undergoing silane coupling agent grafting modification, sodium ion modification and ionic flame retardant liquid modification.

[0008] Preferably, the silane coupling agent includes one or more of 3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-thiolpropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, and vinyltri-tert-butylperoxide silane; And / or, the ionic flame retardant liquid includes one or more of 1-allyl-3-methylimidazolium ammonium chloride, 3-hexyl-1-methyl-1-imidazolium-3-ammonium bromide, and 1-allyl-3-methylimidazolium tetrafluoroborate.

[0009] Preferably, the weight percentage of vinyl contained in the double-terminated vinyl silicone oil is 0.1% to 0.8%; And / or, the double-terminated vinyl silicone oil comprises double vinyl-terminated polydimethylsiloxane.

[0010] Preferably, the hydrogen-containing silicone oil is selected from terminal hydrogen-containing silicone oil and side hydrogen-containing silicone oil. In the B component, the terminal hydrogen-containing silicone oil is 20 to 30 parts, and the side hydrogen-containing silicone oil is 1 to 20 parts; The hydrogen content of the side hydrogen-containing silicone oil is 0.27-1.25%, and the side hydrogen-containing silicone oil includes methyl-terminated side hydrogen silicone oil; The hydrogen content of the terminal hydrogen-containing silicone oil is 0.01% to 0.5%; The terminal hydrogen-containing silicone oil includes double-terminal hydrogen-containing silicone oil.

[0011] Preferably, the thermally conductive filler includes one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, graphene, carbon nanotubes, carbon fiber powder, aluminum hydroxide and magnesium hydroxide; And / or, the catalyst comprises a platinum catalyst.

[0012] On the other hand, the present application also provides a method for preparing the flame-retardant organic silicone two-component thermally conductive potting adhesive described above, comprising the following steps: 40-60 parts of double-terminal vinyl silicone oil, 16-25 parts of modified vermiculite, 120-180 parts of thermal conductive filler and 0.1-0.5 parts of catalyst are mixed uniformly to obtain component A; 21-50 parts of hydrogenated silicone oil, 30-50 parts of double-terminated vinyl silicone oil, 16-25 parts of modified vermiculite and 120-180 parts of thermal conductive filler are uniformly mixed to obtain component B; The component A and the component B are uniformly mixed in a mass ratio of 1:1, and cured to obtain the flame-retardant organic silicone two-component thermally conductive potting adhesive.

[0013] Preferably, the modified vermiculite is prepared by the following method: The solvent and the silane coupling agent are mixed at a first heating temperature, and vermiculite is added for a second heating and stirring, and then a first post-treatment is performed to obtain grafted modified vermiculite; The grafted modified vermiculite is added into the sodium salt solution and mixed and stirred, and then a second post-treatment is performed to obtain sodium vermiculite; The sodium vermiculite and the ionic flame retardant liquid are mixed, and heated and stirred for the third time, and then post-treated for the third time to obtain the modified vermiculite.

[0014] Preferably, the first heating temperature is 30-50°C; The mass ratio of the silane coupling agent to the vermiculite is 1:(2-4); The solvent includes deionized water and an alcohol solvent; the heating temperature of the second heating and stirring is 50-70° C., and the heating time of the second heating and stirring is 1-3 hours; The first post-treatment comprises the following steps: cooling, first standing, first filtering, first washing and first vacuum drying are sequentially performed after the second heating and stirring to obtain the grafted modified vermiculite; The first vacuum drying temperature is 50-70°C, and the first vacuum drying time is 2-8h; The first standing time is 5 to 10 hours.

[0015] Preferably, the sodium salt solution comprises an inorganic sodium salt, and the inorganic sodium salt comprises one or more of sodium chloride, sodium sulfate, and sodium nitrate; The molar concentration of the sodium salt solution is 1-2 mol / L; In each liter of the sodium salt solution, the mass ratio of the sodium ions to the grafted modified vermiculite is (23-46): (50-60); The mixing time of the mixing is 2 to 4 hours; The second post-treatment comprises the following steps: after the mixing and stirring is completed, a second filtration, a second washing and a second vacuum drying are performed in sequence to obtain the sodium vermiculite; The second vacuum drying temperature is 50-70° C., and the second vacuum drying time is 2-4 hours.

[0016] Preferably, the mass ratio of the sodium vermiculite to the ionic flame retardant liquid is 1:(1.2-1.6); The heating temperature of the third heating and stirring is 50-60° C., and the heating time of the third heating and stirring is 4-6 hours; The third post-treatment comprises the following steps: after the third heating and stirring, sequentially performing a second standing, a third filtering, a third washing and a third vacuum drying to obtain the modified vermiculite; The third vacuum drying temperature is 50-70°C, and the third vacuum drying time is 4-6h; The second standing time is 5 to 12 hours.

[0017] The flame-retardant organic silicon two-component thermal conductive potting adhesive provided by the present application comprises modified vermiculite, which is firstly modified by grafting with a silane coupling agent, thereby improving the interfacial adhesion and making the vermiculite better dispersed in the organic silicon resin phase, thereby avoiding the problems of agglomeration and sedimentation of the vermiculite in the organic silicon two-component thermal conductive potting adhesive system; then the vermiculite is modified with sodium ions, which is helpful for a cation exchange reaction with an ionic flame retardant liquid, and is beneficial for modifying the vermiculite with an ionic flame retardant liquid; after the vermiculite is modified with an ionic flame retardant liquid, the flame retardancy of the vermiculite is further improved, and the limiting oxygen index can be further improved. In the silicone two-component thermally conductive potting glue, 16 to 25 parts of modified vermiculite are added to both component A and component B. The total mass content of the modified vermiculite in the potting glue is about 3 to 6%. The amount of modified vermiculite added is small. When the same amount is added, compared with adding other flame retardants, the limiting oxygen index of the thermally conductive potting glue can be improved, and the flame retardant properties of the thermally conductive potting glue can be further improved; at the same time, only 3 to 6wt% of the modified vermiculite is added. A small amount of modified vermiculite can achieve a good flame retardant effect without reducing the amount of thermally conductive filler added and affecting the thermal conductivity of the silicone two-component thermally conductive potting glue. The silicone two-component thermally conductive potting glue has high thermal conductivity, good flame retardant effect, and no sedimentation. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0019] In order to illustrate the technical solution of the present invention, specific embodiments are provided below for illustration.

[0020] In one embodiment of the present application, a flame retardant organic silicone two-component thermally conductive potting adhesive comprises component A and component B, which are measured in parts by weight. The component A comprises 40-60 parts of double-end vinyl silicone oil, 16-25 parts of modified vermiculite, 120-180 parts of thermal conductive filler, and 0.1-0.5 parts of catalyst; The B component includes 21 to 50 parts of hydrogenated silicone oil, 30 to 50 parts of double-terminal vinyl silicone oil, 16 to 25 parts of modified vermiculite, and 120 to 180 parts of thermal conductive filler; The modified vermiculite is obtained by sequentially undergoing silane coupling agent grafting modification, sodium ion modification and ionic flame retardant liquid modification.

[0021] Specifically, double-ended vinyl silicone oil refers to silicone oil containing vinyl groups at both ends, that is, double-terminated vinyl silicone oil; siloxane with a vinyl group at each end of the molecular chain has strong reactivity and is easy to react with Si-H in hydrogen-containing silicone oil to generate a network structure, thereby realizing the curing of the potting compound.

[0022] Vermiculite is formed by the alteration of biotite, iron-bearing mica, chlorite, pyroxene or other similar minerals under the action of weathering, hydrothermal action, groundwater infiltration or a combination of the three. Although its formation varies due to different geological conditions, its morphology and structure may vary to a certain extent, but it is basically composed of SiO 2 (37%~42%), MgO (11%~23%), Al 2 O 3 (9%~17%), Fe 2 O 3 , (5%~18%) and H 2 O (1%~5%), as well as a small amount of Ti, Cr, Li and Ni. Vermiculite is a layered 2:1 hydrated silicate mineral, consisting of two layers of silicon-oxygen tetrahedrons and a layer of magnesium-oxygen octahedrons in the middle. 4+ and Al 3+ It is easily replaced by low-valent ions, making the surface of vermiculite negatively charged. In order to balance the negative charge, Na + , Ca 2 + Mg 2+ The cations are adsorbed between the layers. The layered structure of vermiculite is relatively stable and will not be destroyed by high temperature. Its melting point is greater than 1300℃ and it has excellent heat resistance. Therefore, vermiculite is a common high temperature resistant filler. The expansion property is a unique property of vermiculite. When heated, the interlayer water of vermiculite will quickly vaporize into water vapor to generate high pressure, forcing the vermiculite sheets to separate from each other and forming a porous expansion material in a direction perpendicular to the sheets. This property can be well used to improve the flame retardant properties of adhesives.

[0023] Vermiculite is an inorganic mineral, and its surface contains a large amount of -OH, which is hydrophilic and has poor compatibility with the organic thermal conductive potting glue system. When more vermiculite is added, the stability of the organic thermal conductive potting glue system is easily destroyed, affecting the uniform dispersion of vermiculite in the organic thermal conductive potting glue system, causing the vermiculite to settle, and affecting the sizing effect. Therefore, the inventors have found that the vermiculite can be modified, the amount of vermiculite added can be reduced, and the uniform dispersion of vermiculite in the organic thermal conductive potting glue system can be achieved, thereby avoiding the vermiculite settling phenomenon.

[0024] The modified vermiculite is obtained by sequentially undergoing silane coupling agent grafting modification, sodium ion modification and ionic flame retardant liquid modification, that is, the vermiculite is firstly grafted with a silane coupling agent, then subjected to sodium ion modification after the grafting modification, and then subjected to ionic flame retardant liquid modification after the sodium ion modification.

[0025] Vermiculite is grafted and modified with silane coupling agent. Silane coupling agent is a low molecular weight organosilicon compound containing organic groups and hydrolyzable groups. One end of the hydrolyzable group in the molecule is connected to the surface of the vermiculite, and the organic group at the other end has good bonding with the silicone resin. It can form a "molecular bridge" to improve the interaction between inorganic and polymer molecules, improve compatibility, and make the vermiculite better dispersed in the silicone resin phase, avoiding the agglomeration and sedimentation problems of vermiculite in the silicone two-component thermal conductive potting system. After the vermiculite is grafted and modified with silane coupling agent, it is modified with sodium ions. The introduction of sodium ions in vermiculite helps to react with ionic flame retardant liquids to undergo cation exchange reactions, which is beneficial to the modification of vermiculite with ionic flame retardant liquids. After the vermiculite is modified with ionic flame retardant liquids, the flame retardancy of the vermiculite is further improved, and the limiting oxygen index can be further improved.

[0026] The flame-retardant organic silicon two-component thermal conductive potting adhesive provided by the present application comprises modified vermiculite, which is firstly modified by grafting with a silane coupling agent, thereby improving the interfacial adhesion and making the vermiculite better dispersed in the organic silicon resin phase, thereby avoiding the problems of agglomeration and sedimentation of the vermiculite in the organic silicon two-component thermal conductive potting adhesive system; then the vermiculite is modified with sodium ions, which is helpful for a cation exchange reaction with an ionic flame retardant liquid, and is beneficial for modifying the vermiculite with an ionic flame retardant liquid; after the vermiculite is modified with an ionic flame retardant liquid, the flame retardancy of the vermiculite is further improved, and the limiting oxygen index can be further improved. In the silicone two-component thermally conductive potting glue, 16 to 25 parts of modified vermiculite are added to both component A and component B. The total mass content of the modified vermiculite in the potting glue is about 3 to 6%. The amount of modified vermiculite added is small. When the same amount is added, compared with adding other flame retardants, the limiting oxygen index of the thermally conductive potting glue can be improved, and the flame retardant properties of the thermally conductive potting glue can be further improved; at the same time, only 3 to 6wt% of the modified vermiculite is added. A small amount of modified vermiculite can achieve a good flame retardant effect without reducing the amount of thermally conductive filler added and affecting the thermal conductivity of the silicone two-component thermally conductive potting glue. The silicone two-component thermally conductive potting glue has high thermal conductivity, good flame retardant effect, and no sedimentation.

[0027] The flame-retardant organic silicon two-component thermally conductive potting adhesive provided in the present application has a modified vermiculite which can achieve a flame-retardant effect when added in a relatively small amount, and can simultaneously meet the effects of thermal conductivity and flame-retardant properties.

[0028] In some embodiments, the hydrogen-containing silicone oil is selected from terminal hydrogen-containing silicone oil and side hydrogen-containing silicone oil. In the B component, the terminal hydrogen-containing silicone oil is 20 to 30 parts, and the side hydrogen-containing silicone oil is 1 to 20 parts; Specifically, 1 to 20 parts of side hydrogen-containing silicone oil are added to component B. Adding the side hydrogen-containing silicone oil helps to form a cross-linked network, provide a certain physical strength for the organic silicone two-component thermal conductive potting adhesive, and improve the overall strength of the potting adhesive.

[0029] Add 20-30 parts of terminal hydrogen silicone oil to component B. Terminal hydrogen silicone oil is a polysiloxane that uses the Si-H bond on its terminal group to introduce a silicon-hydrogen bond at the end of the chain through a siliconization reaction. The silicon-hydrogen bond (Si-H) in the terminal hydrogen silicone oil can undergo an addition reaction with the double-terminal vinyl silicone oil under the action of a platinum catalyst, thereby achieving curing and forming a three-dimensional network structure, giving the potting compound good mechanical properties and electrical insulation properties.

[0030] In some embodiments, the hydrogen content in the hydrogen-containing silicone oil is 0.27% to 1.25%.

[0031] The hydrogen content refers to the mass fraction of active hydrogen in the side hydrogen silicone oil. The hydrogen content of the added side hydrogen silicone oil is 0.27~1.25%, which helps to crosslink with the double-terminal vinyl silicone oil to form a network and increase the mechanical strength and thermal stability of the potting compound.

[0032] In some embodiments, the pendant hydrogen-containing silicone oil includes a terminal methyl pendant hydrogen silicone oil.

[0033] In some preferred embodiments, the terminal methyl side hydrogen-containing silicone oil includes one or more of RH-H502 of Ningbo Runhe, RH-H503 of Ningbo Runhe, and RH-H510 of Ningbo Runhe.

[0034] In some embodiments, the weight percentage of vinyl contained in the double-terminal vinyl silicone oil is 0.2% to 0.8%.

[0035] Specifically, the vinyl mass percentage in the double-terminal vinyl silicone oil is in the range of 0.1% to 0.8%, which is helpful to participate in the curing reaction with the side hydrogen-containing silicone oil to form a stable three-dimensional cross-linked network structure.

[0036] In some embodiments, the dual-terminated vinyl silicone oil includes dual-vinyl-terminated polydimethylsiloxane.

[0037] In some preferred embodiments, the double-ended vinyl silicone oil includes one or more of RH-Vi304 of Ningbo Runhe, RH-Vi320 of Ningbo Runhe, MP300 of Sibao Technology, MP450 of Sibao Technology, CX-352-500 of Chensi Technology, and CX-352-300 of Chensi Technology.

[0038] Choosing the above types of double-ended vinyl silicone oil can help reduce the viscosity of the potting compound, improve the fluidity and overall thermal conductivity of the potting compound, improve the heat dissipation efficiency, and improve the durability, weather resistance and stability of the potting compound.

[0039] In some embodiments, the hydrogen content of the hydrogen-terminated silicone oil is 0.01% to 0.5%.

[0040] Specifically, the hydrogen content of the terminal hydrogenated silicone oil is in the range of 0.01% to 0.5%, which helps to improve the hardness of the potting compound.

[0041] In some embodiments, the hydrogen-terminated silicone oil includes a double-terminated hydrogen-terminated silicone oil.

[0042] In some preferred embodiments, the end hydrogen-containing silicone oil includes one or more of CX-350D of Chensi Technology, CR-F22T of Jiangxi Kerui, and IOTA616 of Anhui Aiyota.

[0043] The above-mentioned types of terminal hydrogen-containing silicone oil are selected. The terminal hydrogen-containing silicone oil can act as a cross-linking agent, participate in the vulcanization process, and react with the double-terminal vinyl silicone oil to form a silicon-oxygen bond, thereby connecting the two silicone oil molecules, improving the mechanical strength, flexibility, thermal stability, durability and weather resistance of the potting compound, and improving the heat dissipation efficiency of the potting compound.

[0044] In some embodiments, the thermally conductive filler includes one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, graphene, carbon nanotubes, carbon fiber powder, aluminum hydroxide, and magnesium hydroxide.

[0045] Specifically, the thermally conductive filler is selected from the above types to play a role in thermal conductivity.

[0046] In some embodiments, the catalyst comprises a platinum catalyst.

[0047] Specifically, the platinum catalyst helps to catalyze the reaction of side hydrogen-containing silicone oil, terminal hydrogen-containing silicone oil and double-terminal vinyl silicone oil, thereby increasing the reaction rate.

[0048] The platinum catalyst includes platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane.

[0049] Furthermore, the platinum catalyst includes one or more of CX-5001 of Chensi Technology, ACS-Pt of Sibao Technology, and platinum catalysts produced by Betley Corporation.

[0050] In a second aspect, the present application provides a method for preparing the flame-retardant organic silicone two-component thermally conductive potting adhesive described above, comprising the following steps: 40-60 parts of double-terminal vinyl silicone oil, 16-25 parts of modified vermiculite, 120-180 parts of thermal conductive filler and 0.1-0.5 parts of catalyst are mixed uniformly to obtain component A; 21-50 parts of hydrogenated silicone oil, 30-50 parts of double-terminated vinyl silicone oil, 16-25 parts of modified vermiculite and 120-180 parts of thermal conductive filler are uniformly mixed to obtain component B; The component A and the component B are uniformly mixed in a mass ratio of 1:1, and cured to obtain the flame-retardant organic silicone two-component thermally conductive potting adhesive.

[0051] The present application provides a method for preparing a flame-retardant organic silicone two-component thermally conductive potting adhesive. First, component A and component B are prepared. Then, component A and component B are mixed and cured to obtain the flame-retardant organic silicone two-component thermally conductive potting adhesive. The preparation method is simple. A small amount of modified vermiculite is added to the prepared flame-retardant organic silicone two-component thermally conductive potting adhesive, which can improve the limiting oxygen index of the organic silicone two-component thermally conductive potting adhesive and further improve the flame retardant performance of the thermally conductive potting adhesive system. A small amount of modified vermiculite is added, which does not reduce the amount of thermally conductive filler added and still does not affect the thermal conductivity of the organic silicone two-component thermally conductive potting adhesive. The organic silicone two-component thermally conductive potting adhesive has high thermal conductivity and good flame retardant effect.

[0052] In some embodiments, the curing temperature is 50-70° C., and the curing time is 2-3 hours.

[0053] Specifically, the curing temperature can be 50°C, 52°C, 55°C, 57°C, 60°C, 63°C, 65°C, 68°C, 70°C, etc., as long as the curing temperature is within the range of 50-70°C. The curing temperature and curing time within the above range are conducive to the catalytic polymerization reaction of the double-terminal vinyl silicone oil and the terminal hydrogen silicone oil and the side hydrogen silicone oil to prepare a flame-retardant organic silicone two-component thermal conductive potting adhesive.

[0054] In some embodiments, the hydrogen-containing silicone oil is selected from terminal hydrogen-containing silicone oil and side hydrogen-containing silicone oil. In the B component, the terminal hydrogen-containing silicone oil is 20-30 parts, and the side hydrogen-containing silicone oil is 1-20 parts.

[0055] In some embodiments, the modified vermiculite is prepared by the following method: The solvent and the silane coupling agent are mixed at a first heating temperature, and vermiculite is added for a second heating and stirring, and then a first post-treatment is performed to obtain grafted modified vermiculite; The grafted modified vermiculite is added into the sodium salt solution and mixed and stirred, and then a second post-treatment is performed to obtain sodium vermiculite; The sodium vermiculite and the ionic flame retardant liquid are mixed, and heated and stirred for the third time, and then post-treated for the third time to obtain the modified vermiculite.

[0056] Specifically, the preparation method of modified vermiculite is to first modify the vermiculite with a silane coupling agent to obtain grafted modified vermiculite, enhance the compatibility of vermiculite with an organic matrix, improve the dispersion uniformity of the modified vermiculite in a two-component silicone thermal conductive potting adhesive, and prevent vermiculite from settling. Then, the grafted modified vermiculite is added to a sodium salt solution containing sodium ions to perform sodium ion modification to obtain sodium vermiculite. The surface of the sodium vermiculite contains sodium ions, which is conducive to a cation exchange reaction with an ionic flame retardant liquid, and is conducive to the modification of the vermiculite with an ionic flame retardant liquid. Finally, the sodium vermiculite and the ionic flame retardant liquid are mixed, and the sodium ions react with the ionic flame retardant liquid so that the surface contains flame retardant groups, thereby improving the flame retardant properties of the vermiculite.

[0057] In some embodiments, the silane coupling agent includes one or more of 3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-thiolpropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, and vinyltri-tert-butylperoxide silane.

[0058] Specifically, the silane coupling agent is selected from the above-mentioned types, containing organic groups and hydrolyzable groups. The hydrolyzable groups (such as Si-OR) in the silane coupling agent are hydrolyzed in water to form silanol (Si-OH), and then form hydrogen bonds with -OH on the surface of vermiculite. The non-hydrolyzable groups in the silane coupling agent, such as amino, vinyl, etc., can react with silicone resins such as double-terminal vinyl silicone oil, terminal hydrogen-containing silicone oil, and side hydrogen-containing silicone oil to enhance the compatibility of vermiculite with organic matrices, improve the dispersion uniformity of modified vermiculite in silicone two-component thermal conductive potting adhesive, and prevent vermiculite from settling.

[0059] In some preferred embodiments, the silane coupling agent is γ-aminopropyltriethoxysilane.

[0060] In some embodiments, the ionic flame retardant liquid includes one or more of 1-allyl-3-methylimidazolium ammonium chloride, 3-hexyl-1-methyl-1-imidazolium-3-ammonium bromide, and 1-allyl-3-methylimidazolium tetrafluoroborate.

[0061] Specifically, directly introducing flame-retardant ionic liquids into the system often results in precipitation or phase separation. After the vermiculite is modified by ionic liquids, the ionic liquids can form a stable structure with the vermiculite and capture gas-phase free radicals or promote the formation of a condensed carbon layer to enhance the flame retardant properties.

[0062] In some embodiments, the solvent includes deionized water and an alcohol solvent; the mass ratio of the deionized water to the alcohol solvent is (30-70): (70-30).

[0063] Alcohol solvents include ethanol, propanol, butanol, pentanol and the like.

[0064] Water and alcohol solvents are used as solvents. Water is a necessary medium for the hydrolysis of the hydrolyzable groups in the silane coupling agent. Since the solubility of some silane coupling agents in water is limited, alcohol solvents are added to increase the solubility of the silane coupling agent. The mass ratio of deionized water and alcohol solvent is in the range of (30~70): (70~30), which is helpful to dissolve the silane coupling agent.

[0065] The first heating temperature is 30-50°C.

[0066] Specifically, mixing the solvent and the silane coupling agent at the first heating temperature specifically includes the following steps: mixing deionized water, an alcohol solvent and the silane coupling agent, and heating them in a water bath at the first heating temperature.

[0067] The first heating temperature is in the range of 30-50° C. to promote the hydrolysis of the silane coupling agent. The heating time under the condition of the first heating temperature is 1-2 hours.

[0068] In some embodiments, the mass ratio of the silane coupling agent to the vermiculite is 1:(2-4).

[0069] Specifically, limiting the mass ratio of the silane coupling agent to the vermiculite to a range of 1:(2-4) is helpful for the adsorption and diffusion of the silane coupling agent on the surface of the vermiculite, thereby improving the modification effect of the vermiculite.

[0070] In some embodiments, the heating temperature of the second heating and stirring is 50-70° C., and the heating time of the second heating and stirring is 1-3 h.

[0071] Specifically, vermiculite is added for a second heating and stirring, and the added vermiculite is vermiculite that has been treated with impurities removal, wherein the impurity removal step refers to the prior art, and impurities on the surface of the vermiculite can be removed by washing with deionized water. The second heating and stirring refers to stirring while heating, the heating temperature is 50-70°C, and the heating time is 1-3 hours. Heating promotes the hydrolysis of the silane coupling agent, activates the hydroxyl groups on the surface of the vermiculite, and makes the vermiculite more easily react with the silanol generated after the hydrolysis of the silane coupling agent; stirring during the heating process helps the vermiculite to fully contact with the silane coupling agent and promote the reaction.

[0072] In some embodiments, the first post-treatment comprises the following steps: cooling, first standing, first filtering, first washing and first vacuum drying are sequentially performed after the second heating and stirring to obtain the grafted modified vermiculite; The first vacuum drying temperature is 50-70°C, and the first vacuum drying time is 2-8h; The first standing time is 5 to 10 hours.

[0073] Specifically, the cooling method can be natural cooling or cooling with circulating water to room temperature (25±5°C); after cooling to room temperature, the first standing is performed at room temperature to allow the silane coupling agent to have more time to be adsorbed on the vermiculite surface, thereby improving the uniformity of the modification effect.

[0074] The first filtration includes suction filtration. Since vermiculite is generally in powder form, suction filtration is directly used to extract the solvent, and the remaining vermiculite is modified by the silane coupling agent.

[0075] The first washing includes washing the vermiculite modified with the silane coupling agent with deionized water to remove the unreacted silane coupling agent on the surface. The purpose of the first vacuum drying is to remove the deionized water and the like on the surface of the vermiculite modified with the silane coupling agent.

[0076] In some embodiments, the sodium salt solution includes an inorganic sodium salt, and the inorganic sodium salt includes one or more of sodium chloride, sodium sulfate, and sodium nitrate; The molar concentration of the sodium salt solution is 1-2 mol / L.

[0077] Specifically, the sodium salt solution refers to a solution obtained by uniformly mixing an inorganic sodium salt and deionized water. The inorganic sodium salt is selected from the above types, and the molar concentration is in the range of 1-2 mol / L. The cation contained is sodium ion. The grafted modified vermiculite is placed in the sodium salt solution, and the sodium ions are adsorbed on the surface of the grafted modified vermiculite to obtain sodium vermiculite.

[0078] The molar concentration of the sodium salt solution can be 1 mol / L, 1.1 mol / L, 1.3 mol / L, 1.5 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L, 2.0 mol / L, etc., as long as the molar concentration of the sodium salt solution is within the range of 1 to 2 mol / L.

[0079] In some embodiments, in each liter of the sodium salt solution, the mass ratio of the sodium ions to the grafted modified vermiculite is (23-46): (50-60); and the mixing time of the mixing is 2-4 hours.

[0080] Specifically, the molar concentration of the sodium salt solution is 1-2 mol / L, the content of sodium ions per liter of sodium salt solution is 1-2 mol, the mass of sodium ions is 23-46 g, and the mass ratio of the mass of sodium ions per liter of sodium salt solution to the mass of the grafted modified vermiculite is (23-46): (50-60), indicating that the mass of the grafted modified vermiculite added per liter of sodium salt solution is 50-60 g, which helps to evenly disperse the sodium ions and adsorb them on the surface of the grafted modified vermiculite to obtain sodium vermiculite, which is beneficial to the subsequent adsorption of more flame retardant groups on the surface of the sodium vermiculite.

[0081] After adding the grafted modified vermiculite to the sodium salt solution, stirring at room temperature for 2 to 4 hours is conducive to the full contact between the sodium ions and the grafted modified vermiculite, so that the sodium ions are uniformly adsorbed on the surface of the grafted modified vermiculite. The stirring time can be 2 hours, 2.5 hours, 3.0 hours, 3.5 hours, 4.0 hours, etc., as long as the stirring time is 2 to 4 hours.

[0082] In some embodiments, the second post-treatment comprises the following steps: after the mixing and stirring is completed, a second filtration, a second washing and a second vacuum drying are performed in sequence to obtain the sodium vermiculite; The second vacuum drying temperature is 50-70° C., and the second vacuum drying time is 2-4 hours.

[0083] Specifically, after the mixing and stirring is completed, a second filtration is performed to obtain vermiculite modified with sodium ions, and then the sodium ion-modified vermiculite is washed for a second time with deionized water to remove anions of the inorganic sodium salt; after the second washing is completed, a second vacuum drying is performed, the second vacuum drying temperature is 50-70° C., and the second vacuum drying time is 2-4 hours, so as to remove the deionized water on the surface and obtain the sodium vermiculite.

[0084] In some embodiments, the mass ratio of the sodium vermiculite to the ionic flame retardant liquid is 1:(1.2-1.6).

[0085] Specifically, sodium vermiculite and ionic flame retardant liquid are mixed, and the mass ratio of sodium vermiculite to ionic flame retardant liquid is limited to 1: (1.2~1.6) range, which helps the sodium ions on the surface of the sodium vermiculite to react with the anions in the ionic flame retardant liquid, so that the flame retardant groups are adsorbed on the surface of the sodium vermiculite, thereby improving the flame retardant effect of the modified vermiculite.

[0086] Specifically, the mass ratio of sodium vermiculite to the ionic flame retardant liquid can be 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, etc., as long as the mass ratio of sodium vermiculite to the ionic flame retardant liquid is within the range of 1:(1.2~1.6).

[0087] In some embodiments, the heating temperature of the third heating and stirring is 50-60° C., and the heating time of the third heating and stirring is 4-6 hours.

[0088] Specifically, after the sodium vermiculite and the ionic flame retardant liquid are mixed, heating and stirring are performed for the third time, the heating temperature is 50-60° C., and the heating time is 4-6 hours, which helps to improve the reaction between the sodium ions and the ionic flame retardant liquid and improve the reaction rate.

[0089] In some embodiments, the third post-treatment comprises the following steps: after the third heating and stirring, sequentially performing a second standing, a third filtering, a third washing and a third vacuum drying to obtain the modified vermiculite; The third vacuum drying temperature is 50-70°C, and the third vacuum drying time is 4-6h; The second standing time is 5 to 12 hours.

[0090] Specifically, the second standing time is 5 to 12 hours, in order to increase the reaction time of the sodium ions and the ionic flame retardant liquid. After the second standing, the third filtration is performed, and the filtration is preferably suction filtration to remove the excess ionic flame retardant liquid, and the remaining sodium vermiculite modified by the ionic flame retardant liquid is washed for the third time, such as using deionized water for the third washing, to remove the unreacted ionic flame retardant liquid on the surface of the vermiculite, and the third vacuum drying is performed after the third washing, the vacuum drying temperature is 50 to 70°C, the third vacuum drying time is 4 to 6 hours, and the modified vermiculite is obtained after the third vacuum drying.

[0091] The present invention is further described below by way of examples.

[0092] Example 1 Preparation of modified vermiculite S1: Preparation of grafted modified vermiculite 200g of ethanol, 110g of deionized water and 40g of silane coupling agent KH550 (γ-aminopropyltriethoxysilane) were weighed and added to a flask for mixing, and the mixture was placed in a water bath at a first heating temperature of 40°C for 1h; 150g of refined vermiculite was weighed and placed in a flask in a water bath for a second heating and stirring, the heating temperature of the second heating and stirring was 60°C, and the second heating and stirring time was 2h, that is, after constant temperature stirring at 60°C for 2h, the flask was taken out, and after natural cooling, the mixture was allowed to stand for a first time at room temperature for 10h, and after the first standing, the first suction filtration was performed; after the first suction filtration, the first washing was performed with deionized water, and the vermiculite treated with the silane coupling agent was rinsed several times to remove the unreacted silane coupling agent KH550; after the first washing, the first vacuum drying was performed, and the first vacuum drying step was to place the vermiculite after the first washing in a 50-70°C drying oven for vacuum drying for 4h to constant weight, and then cooled to room temperature to obtain the grafted modified vermiculite.

[0093] S2: Preparation of sodium vermiculite Prepare 1L of 1mol / L sodium chloride solution and place it in a flask. Add 60g of grafted modified vermiculite into the three-necked flask and stir at room temperature for 3h before taking out the flask. Then perform a second filtration and use a circulating water pump to remove the sodium chloride solution. Then perform a second washing, that is, rinse with deionized water 3 times to remove the Cl in the system.- After the second washing, a second vacuum drying is performed, the second vacuum drying temperature is 60° C., the second vacuum drying time is 3 hours, and the sodium vermiculite is obtained. In each liter of the sodium salt solution, the mass ratio of the sodium ions to the grafted modified vermiculite is 23:60.

[0094] S3: Preparation of modified vermiculite Weigh sodium vermiculite and ionic flame retardant liquid 1-allyl-3-methylimidazolium chloride, the mass ratio of sodium vermiculite to 1-allyl-3-methylimidazolium chloride is 1:1.4, put them into a flask for the third heating and stirring, the heating temperature of the third heating and stirring is 60℃, and the heating time of the third heating and stirring is 4h. After the third heating and stirring, the second standing is carried out, and the second standing time is 8h; after the second standing, the third suction filtration is carried out, and the excess 1-allyl-3-methylimidazolium chloride is removed by using a circulating water pump. After the third suction filtration, the third washing is carried out, that is, rinsing with deionized water 3 times to remove the excess 1-allyl-3-methylimidazolium chloride in the system. After the third washing, the third vacuum drying is carried out. The third vacuum drying step is to vacuum dry the sodium vermiculite modified by 1-allyl-3-methylimidazolium chloride at 70℃, and the third vacuum drying time is 4h to obtain modified vermiculite.

[0095] S4: Preparation of flame-retardant silicone two-component thermally conductive potting compound 50 parts of double-terminal vinyl silicone oil (CX-352-500 of Chensi Technology), 20 parts of the modified vermiculite prepared above, 150 parts of thermal conductive filler alumina and 0.5 parts of Custer catalyst (platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane) were mixed evenly to obtain component A; 25 parts of terminal hydrogen silicone oil (CX-350D of Chensi Technology), 50 parts of double-terminal vinyl silicone oil (CX-352-500 of Chensi Technology), 10 parts of side hydrogen silicone oil (RH-H502 of Ningbo Runhe), 20 parts of the modified vermiculite prepared above and 150 parts of thermal conductive filler alumina are mixed evenly to obtain component B; The component A and the component B are mixed evenly in a mass ratio of 1:1, poured into a mold and cured at 60° C. for 2.5 hours to obtain the flame-retardant organic silicone two-component thermally conductive potting adhesive.

[0096] Example 2 Most of the steps in this embodiment are the same as those in Embodiment 1, except that the heating temperature of the second heating and stirring in step S1 is 65° C., and the time of the second heating and stirring is 2 h; the rest are the same as in Embodiment 1.

[0097] Example 3 Most of the steps in this embodiment are the same as those in Embodiment 1, except that the heating temperature of the second heating and stirring in step S1 is 75° C., and the time of the second heating and stirring is 5 h; the rest is the same as in Embodiment 1.

[0098] Example 4 Most of the steps of this embodiment are the same as those of embodiment 1, except that in step S1, the silane coupling agent is vinyl tri-tert-butyl peroxide silane, the amount of vinyl tri-tert-butyl peroxide silane added is 75 g, and the amount of vermiculite added is 150 g.

[0099] Example 5 Most of the steps of this embodiment are the same as those of embodiment 1, except that in step S2, 1 L of 1.5 mol / L sodium chloride solution is prepared, the mass ratio of sodium ions to the mass of grafted modified vermiculite is 34.5:60, and the rest is the same as embodiment 1.

[0100] Example 6 Most of the steps of this embodiment are the same as those of Embodiment 5, except that in step S2, 1 L of 0.2 mol / L sodium chloride solution is prepared, the mass ratio of sodium ions to the mass of grafted modified vermiculite is 4.6:60, and the rest is the same as Embodiment 5.

[0101] Example 7 Most of the steps of this embodiment are the same as those of Example 1, except that: in step S3, the heating temperature of the third heating and stirring is 60° C., and the time of the second heating and stirring is 6 h; the mass ratio of sodium vermiculite to 1-allyl-3-methylimidazolium chloride is 1:1.2; and the rest is the same as Example 1.

[0102] Example 8 Most of the steps of this embodiment are the same as those of Embodiment 1, except that in step S3, the mass ratio of sodium vermiculite to 1-allyl-3-methylimidazolium chloride is 1:1.6; the rest is the same as that of Embodiment 1.

[0103] Example 9 Most of the steps of this embodiment are the same as those of embodiment 1, except that in step S3, the mass ratio of sodium vermiculite to 1-allyl-3-methylimidazolium chloride is 1:2.0; the rest is the same as embodiment 1.

[0104] Example 10 Most of the steps of this embodiment are the same as those of Embodiment 1, except that in step S3, the mass ratio of sodium vermiculite to 1-allyl-3-methylimidazolium chloride is 1:1; the rest is the same as that of Embodiment 1.

[0105] Embodiment 11 Most of the steps in this embodiment are the same as those in Embodiment 1, except that in step S3, the heating temperature of the third heating and stirring is 20° C., and the time of the second heating and stirring is 2 h; the rest are the same as in Embodiment 1.

[0106] Examples 12 to 19 and Comparative Examples 1 to 7 Most of the steps of Examples 12 to 19 and Comparative Examples 1 to 7 are the same as those of Example 1, except that in step S4, component A and component B are different, as shown in Table 1.

[0107] Table 1 Comparative Example 8 Most of the steps of this comparative example are the same as those of Example 1, except that the preparation method of the modified vermiculite is different; Comparative Example 1 only has step S1, and does not have steps S2 and S3; the rest is the same as Example 1.

[0108] Comparative Example 9 Most of the steps of this comparative example are the same as those of Example 1, except that the preparation method of the modified vermiculite is different; Comparative Example 1 only has steps S1 and S2, but no step S3; the rest are the same as Example 1.

[0109] Comparative Example 10 Most of the steps of this comparative example are the same as those of Example 1, except that the preparation method of the modified vermiculite is different; Comparative Example 1 only has steps S1 and S3, but no step S2; the rest are the same as Example 1.

[0110] Performance Testing The flame-retardant organic silicon two-component thermally conductive potting adhesives prepared in the above-mentioned embodiments and comparative examples were subjected to the following performance tests.

[0111] 1. Limiting oxygen index A standard specimen is prepared from the cured flame-retardant two-component thermal conductive silicone encapsulant, which is placed vertically in a combustion tube. After a certain concentration of oxygen and nitrogen is filled in, the specimen is ignited. The ratio of oxygen to nitrogen is adjusted, and the combustion of the specimen is observed. The oxygen concentration is adjusted according to the combustion of the specimen until the specimen just maintains the minimum oxygen concentration for balanced combustion. The oxygen content is expressed as a percentage after calculation.

[0112] 2. Thermal conductivity The heat flow meter method is a comparative method that uses a calibrated heat flow sensor to measure the heat flow through the sample, and the absolute value of the thermal conductivity is obtained. During the measurement, a sample of a certain thickness is inserted between two plates, and a certain temperature gradient is set. A calibrated heat flow sensor is used to measure the heat flow through the sample, and the sensor is in contact with the sample between the plate and the sample. The thermal conductivity of the sample can be calculated by measuring the thickness of the sample, the temperature gradient between the upper and lower plates, and the heat flow through the sample. The thermal conductivity range of the heat flow method test material is relatively narrow (0.015-5W / m·k), and the temperature range is 90℃ for hot plates and 0℃~70℃ for cold plates.

[0113] 3. Glue application amount The prepared A and B components were divided into 50mL two-component rubber tubes, and placed vertically at room temperature with the rubber outlet facing downward for 7 days before testing. During the test, the rubber liquid was squeezed out through the mixing tube, and the mass of the rubber liquid squeezed out within 10 seconds was weighed on a balance. The thrust used during extrusion was fixed at 200N.

[0114] 4. Flame retardant properties The sample is prepared into a strip with a length of 125mm, a width of 13mm, and a thickness of 1.5mm, and there should be few bubbles on the surface of the sample. The sample is placed in the outer flame of the Bunsen burner and burned. After two 10-second combustion tests on the sample, the residual flame and residual combustion are extinguished within 30 seconds, and the dripping particles cannot ignite the cotton.

[0115] The test results of Example 1 and Examples 2 to 12 are shown in Table 2. The test results of Example 1, Examples 14 to 19 and Comparative Examples 1 to 10 are shown in Table 3.

[0116] Table 2 It can be seen from Table 2 that, in comparison between Example 1 to Example 2 and Example 3, in Example 3, during the grafting modification of vermiculite, the heating temperature of the second heating and stirring is higher than 50-70°C. The possible reason is that the high temperature affects the connection between the silane coupling agent and the vermiculite, affects the fluidity of the potting glue, and further affects the thermal conductivity.

[0117] Comparing Examples 1 and 5 with Example 6, the molar concentration of the sodium salt in Example 6 is lower than 1-2 mol / L, and the sodiumization of the grafted modified vermiculite is incomplete, which affects the modification of the flame retardant ionic liquid. The flame retardant properties of the modified vermiculite are reduced, and the limiting oxygen index is reduced. This indicates that in each liter of the sodium salt solution, the mass ratio of the sodium ions to the grafted modified vermiculite is in the range of (23-46): (50-60), which is helpful for the sodiumization of the vermiculite to be modified with a flame retardant ionic liquid, improve the limiting oxygen index, and improve the flame retardant properties of the thermal conductive potting glue.

[0118] Comparing Examples 1, 7-8 with Examples 9 and 10, in Example 9, the mass ratio of sodium vermiculite to ionic flame retardant liquid is higher than 1: (1.2-1.6), the flame retardant performance will not increase, and the preparation cost will increase; in Example 10, the mass ratio of sodium vermiculite to ionic flame retardant liquid is lower than 1: (1.2-1.6), and the flame retardant performance decreases, indicating that the mass ratio of sodium vermiculite to ionic flame retardant liquid is within the range of 1: (1.2-1.6), which improves the limiting oxygen index and improves the flame retardant performance of the thermal conductive potting glue.

[0119] Comparing Examples 1 and 7 with Example 11, the third stirring temperature in Example 11 is lower than 50-60°C, the limiting oxygen index is reduced, and the flame retardant performance is V1, indicating that the third stirring temperature within the range of 50-60°C is beneficial to the flame retardant modification of sodium vermiculite and the improvement of the flame retardant properties of the thermal conductive potting glue.

[0120] Table 3 It can be seen from Table 3 that by comparing Example 1 with Comparative Examples 3-5, neither component A nor component B in Comparative Example 3 has any flame retardant or flame retardant compound added, the limiting oxygen index is low, and the flame retardancy is poor; the component A and component B in Comparative Example 4 add the same fraction of flame retardant IPPP as in Example 1, although the flame retardant grade meets the standard, the limiting oxygen index is reduced, and the thermal conductivity is lower than that of Example 1; when the amount of flame retardant IPPP is reduced in the component A and group B of Comparative Example 5, the flame retardant grade will not meet the requirements; it indicates that the addition of the modified vermiculite of the present application to the component A and component B can improve the limiting oxygen index, flame retardant performance, and thermal conductivity of the silicone two-component thermally conductive potting glue.

[0121] Comparing Examples 1, 16-19 and 6-7, the modified vermiculite of component A in comparative example 6-7 is not in the range of 16 to 25 parts, and the modified vermiculite of component B is not in the range of 16 to 25 parts. The limiting oxygen index of the prepared thermal conductive potting glue is low and the thermal conductivity is poor. The added modified vermiculite is higher than the range of 16 to 25 parts, and the amount of glue applied is reduced, indicating that too much modified vermiculite is added, and agglomeration and sedimentation may occur in the thermal conductive potting glue system; it indicates that component A and component B meet the range specified in this application, and the silicone two-component thermal conductive potting glue has high thermal conductivity, good flame retardant effect, and no sedimentation problem.

[0122] Comparison between Examples 1, 12-14 and Comparative Examples 1-2 shows that component A includes 40-60 parts of double-ended vinyl silicone oil, 16-25 parts of modified vermiculite, 120-180 parts of thermally conductive filler, and 0.1-0.5 parts of catalyst; component B includes 20-30 parts of end-hydrogenated silicone oil, 30-50 parts of double-ended vinyl silicone oil, 1-20 parts of side-hydrogenated silicone oil, 16-25 parts of modified vermiculite, and 120-180 parts of thermally conductive filler. The prepared silicone two-component thermally conductive potting glue has high limiting oxygen index, flame retardant properties, and thermal conductivity.

[0123] In contrast to Example 1 and Comparative Examples 8-10, in Comparative Example 8, the vermiculite is modified with a silane coupling agent, but the flame retardant grade does not meet the standard and the thermal conductivity is poor; in Comparative Example 9, the vermiculite is modified with a silane coupling agent and a sodium ion, and the obtained potting glue is compared with Comparative Example 8, and the flame retardant grade does not meet the standard, the thermal conductivity is still low, and there is still a sedimentation problem; in Comparative Example 10, the vermiculite is modified with a silane coupling agent and an ionic flame retardant liquid, and because there are no sodium ions on the surface of the vermiculite, the flame retardant grade does not meet the standard and the thermal conductivity is low; This indicates that the modified vermiculite provided by the present application is firstly grafted with a silane coupling agent and then grafted with a silane coupling agent. The modification improves the compatibility, makes the vermiculite better dispersed in the silicone resin phase, avoids the agglomeration and sedimentation problems of the vermiculite in the silicone two-component thermal conductive potting glue system, and then the vermiculite is modified with sodium ions, which is helpful for the cation exchange reaction with the ionic flame retardant liquid, and is beneficial for the ionic flame retardant liquid modification of the vermiculite. After the vermiculite is modified with the ionic flame retardant liquid, the flame retardancy of the vermiculite is further improved, and the limiting oxygen index can be further improved. The prepared flame retardant silicone two-component thermal conductive potting glue has high thermal conductivity, good flame retardancy, and no sedimentation problem.

[0124] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention.

Claims

1. A flame retardant organic silicone two-component thermally conductive potting adhesive, characterized in that: Including component A and component B, in parts by weight, The component A comprises 40-60 parts of double-end vinyl silicone oil, 16-25 parts of modified vermiculite, 120-180 parts of thermal conductive filler, and 0.1-0.5 parts of catalyst; The B component includes 21 to 50 parts of hydrogenated silicone oil, 30 to 50 parts of double-terminal vinyl silicone oil, 16 to 25 parts of modified vermiculite, and 120 to 180 parts of thermal conductive filler; The modified vermiculite is obtained by sequentially undergoing silane coupling agent grafting modification, sodium ion modification and ionic flame retardant liquid modification.

2. The flame-retardant organic silicon two-component thermally conductive potting adhesive according to claim 1, characterized in that: The silane coupling agent includes one or more of 3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-mercaptopropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, and vinyltri-tert-butylperoxide silane; And / or, the ionic flame retardant liquid includes one or more of 1-allyl-3-methylimidazolium ammonium chloride, 3-hexyl-1-methyl-1-imidazolium-3-ammonium bromide, and 1-allyl-3-methylimidazolium tetrafluoroborate.

3. The flame retardant organic silicon two-component thermally conductive potting adhesive according to claim 1, characterized in that: The mass percentage of vinyl contained in the double-terminated vinyl silicone oil is 0.1% to 0.8%; And / or, the double-terminated vinyl silicone oil comprises double vinyl-terminated polydimethylsiloxane.

4. The flame-retardant organic silicon two-component thermally conductive potting adhesive according to claim 1, characterized in that: The hydrogen-containing silicone oil is selected from terminal hydrogen-containing silicone oil and side hydrogen-containing silicone oil. In the B component, the terminal hydrogen-containing silicone oil is 20-30 parts, and the side hydrogen-containing silicone oil is 1-20 parts; The hydrogen content of the side hydrogen-containing silicone oil is 0.27-1.25%, and the side hydrogen-containing silicone oil includes methyl-terminated side hydrogen silicone oil; The hydrogen content of the terminal hydrogenated silicone oil is 0.01% to 0.5%; The terminal hydrogen-containing silicone oil includes double-terminal hydrogen-containing silicone oil.

5. The flame-retardant organic silicon two-component thermally conductive potting adhesive according to claim 1, characterized in that: The thermally conductive filler includes one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, graphene, carbon nanotubes, carbon fiber powder, aluminum hydroxide and magnesium hydroxide; And / or, the catalyst comprises a platinum catalyst.

6. A method for preparing the flame-retardant organic silicon two-component thermally conductive potting adhesive according to any one of claims 1 to 5, characterized in that: The following steps are involved: 40-60 parts of double-terminal vinyl silicone oil, 16-25 parts of modified vermiculite, 120-180 parts of thermal conductive filler and 0.1-0.5 parts of catalyst are mixed uniformly to obtain component A; 21-50 parts of hydrogenated silicone oil, 30-50 parts of double-terminated vinyl silicone oil, 16-25 parts of modified vermiculite and 120-180 parts of thermal conductive filler are uniformly mixed to obtain component B; The component A and the component B are uniformly mixed in a mass ratio of 1:1, and cured to obtain the flame-retardant organic silicone two-component thermally conductive potting adhesive.

7. The method for preparing the flame-retardant organic silicon two-component thermally conductive potting adhesive according to claim 6, characterized in that: The modified vermiculite is prepared by the following method: The solvent and the silane coupling agent are mixed at a first heating temperature, and vermiculite is added for a second heating and stirring, and then a first post-treatment is performed to obtain grafted modified vermiculite; The grafted modified vermiculite is added into the sodium salt solution and mixed and stirred, and then a second post-treatment is performed to obtain sodium vermiculite; The sodium vermiculite and the ionic flame retardant liquid are mixed, and heated and stirred for the third time, and then post-treated for the third time to obtain the modified vermiculite.

8. The method for preparing the flame-retardant organic silicon two-component thermally conductive potting adhesive according to claim 7, characterized in that: The first heating temperature is 30-50°C; The mass ratio of the silane coupling agent to the vermiculite is 1:(2-4); The solvent includes deionized water and alcohol solvent; The heating temperature of the second heating and stirring is 50-70°C, and the heating time of the second heating and stirring is 1-3h; The first post-treatment comprises the following steps: cooling, first standing, first filtering, first washing and first vacuum drying are sequentially performed after the second heating and stirring to obtain the grafted modified vermiculite; The first vacuum drying temperature is 50-70°C, and the first vacuum drying time is 2-8h; The first standing time is 5 to 10 hours.

9. The method for preparing the flame-retardant organic silicon two-component thermally conductive potting adhesive according to claim 7, characterized in that: The sodium salt solution includes an inorganic sodium salt, and the inorganic sodium salt includes one or more of sodium chloride, sodium sulfate, and sodium nitrate; The molar concentration of the sodium salt solution is 1-2 mol / L; In each liter of the sodium salt solution, the mass ratio of the sodium ions to the grafted modified vermiculite is (23-46): (50-60); The mixing time of the mixing is 2 to 4 hours; The second post-treatment comprises the following steps: after the mixing and stirring is completed, a second filtration, a second washing and a second drying are performed in sequence to obtain the sodium vermiculite; The second vacuum drying temperature is 50-70° C., and the second vacuum drying time is 2-4 hours.

10. The method for preparing the flame-retardant organic silicon two-component thermally conductive potting adhesive according to claim 7, characterized in that: The mass ratio of the sodium vermiculite to the ionic flame retardant liquid is 1:(1.2-1.6); The heating temperature of the third heating and stirring is 50-60° C., and the heating time of the third heating and stirring is 4-6 hours; The third post-treatment comprises the following steps: after the third heating and stirring, sequentially performing a second standing, a third filtering, a third washing and a third vacuum drying to obtain the modified vermiculite; The third vacuum drying temperature is 50-70°C, and the third vacuum drying time is 4-6h; The second standing time is 5 to 12 hours.

Citation Information

Patent Citations

  • Ball milling method for preparing organic vermiculite with large layer distance

    CN101850983A

  • Method for modifying vermiculite by using surfactant and application of modified vermiculite

    CN117398967A

  • Sepiolite-based flame-retardant composite material as well as preparation method and application thereof

    CN117964955A

  • Double-component pouring sealant based on modified vermiculite and preparation method thereof

    CN118085806A

  • Organic silicone resin aluminum base copper clad laminate and preparation method thereof

    US20180370189A1

Cited By

  • Flame-retardant epoxy glue and preparation method thereof

    CN119799237A

  • Heat-conducting flame-retardant liquid silicone rubber and preparation method thereof

    CN120554853A