Manganese-based composite abrasive particle with high catalytic activity as well as preparation method and application of manganese-based composite abrasive particle
By using graphene oxide in chemical mechanical polishing to improve the catalytic effect of manganese dioxide and combine it with alumina abrasive particles to form highly catalytically active manganese-based composite abrasive particles, the low surface defect removal rate of silicon carbide in the prior art is solved. The problem is to achieve efficient polishing effect.
Patent Information
- Application Number
- CN202411285606.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, catalysts are limited in the field of chemical mechanical polishing, and cannot further improve the surface defect removal rate and efficiency of silicon carbide wafers.
Graphene oxide significantly improves the catalytic effect of manganese dioxide on potassium permanganate, and combines it with alumina abrasive particles to form highly catalytically active manganese-based composite abrasive particles, which are used to prepare polishing liquid to increase the polishing rate of silicon carbide .
The polishing rate of silicon carbide is significantly improved to reach more than 1000nm/h, and the polishing effect of alumina abrasive particles on silicon carbide is significantly improved.
Smart Images

Figure CN119039936A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of abrasive particles used in polishing liquids, and specifically to a manganese-based composite abrasive particle with high catalytic activity, and a preparation method and application thereof. Background Art
[0002] Power devices with silicon carbide as substrate have a series of excellent properties such as high strength, high hardness, high temperature resistance, and corrosion resistance, so they have been widely used. In recent years, with the further increase in demand for new energy and 5G construction, the market demand for silicon carbide materials has maintained rapid growth, which has put forward higher requirements on the polishing quality of silicon carbide substrates. While removing surface defects such as micro-bumps and micro-scratches on the surface of silicon carbide wafers, the material removal rate of silicon carbide wafers should be maximized.
[0003] At present, potassium permanganate is generally used as an oxidant to polish the surface of silicon carbide wafers using chemical mechanical polishing technology. In order to further increase the material removal rate, adding a suitable catalyst to promote the oxidation rate of silicon carbide wafers by potassium permanganate is very promising. In addition, improving the catalytic effect of the catalyst can also significantly increase the material removal rate. However, the application of catalysts in the field of chemical mechanical polishing in the prior art is limited, and it is impossible to further improve the material removal rate and efficiency of chemical mechanical polishing. Summary of the invention
[0004] The purpose of this experiment is to provide a manganese-based composite abrasive with high catalytic activity and a preparation method and application thereof, wherein graphene oxide significantly improves the catalytic effect of manganese dioxide on potassium permanganate, thereby increasing the polishing rate.
[0005] The present application provides a method for preparing a manganese-based composite abrasive with high catalytic activity, comprising:
[0006] S01: Add solid ice, concentrated sulfuric acid, graphite powder and sodium nitrate into a flask;
[0007] S02: Stir the solution at 5°C, then add potassium permanganate; slowly drip deionized water, raise the temperature to 35°C and keep it for 2 hours;
[0008] S03: heating the mixed solution to 98°C and maintaining for 15 minutes;
[0009] S04: After the mixed solution is cooled to room temperature, a hydrogen peroxide solution is added to the mixed solution to obtain a bright yellow solution;
[0010] S05: washing the bright yellow solution with dilute hydrochloric acid, and then obtaining graphene oxide by a separation method of suction filtration, centrifugation and drying;
[0011] S06: dispersing graphene oxide into deionized water by ultrasonic means, adding manganese sulfate and then dropping potassium permanganate until the solution stops fading, so that manganese dioxide is precipitated on the graphene oxide; adding aluminum oxide abrasive and ultrasonically dispersing the abrasive so that the abrasive is impregnated on the graphene oxide, thereby obtaining manganese-based composite abrasive.
[0012] Furthermore, in step S01, the mass ratio of concentrated sulfuric acid, graphite powder and sodium nitrate is 430:6:3.
[0013] Furthermore, in step S02, the mass ratio of potassium permanganate to deionized water is 9:144.
[0014] Furthermore, the concentration of the hydrogen peroxide solution in step S04 is 30 wt.%, and the mass ratio of the hydrogen peroxide solution to the potassium permanganate in step S02 is 30:9.
[0015] Furthermore, the dilute hydrochloric acid in step S05 is prepared by mixing concentrated hydrochloric acid and deionized water in a volume ratio, the concentration of the concentrated hydrochloric acid is 37wt.%, the volume ratio of concentrated hydrochloric acid to deionized water is 1:3, and the mass ratio of the dilute hydrochloric acid to the deionized water in S02 is 1:1.
[0016] Furthermore, in step S06, the mass ratio of graphene oxide, manganese sulfate and aluminum oxide abrasive is 0.5:0.0521:1.
[0017] The present application provides a manganese-based composite abrasive with high catalytic activity, which is prepared by the preparation method described above.
[0018] The present application provides an application of a manganese-based composite abrasive with high catalytic activity for preparing a polishing liquid for silicon carbide.
[0019] This application has the following beneficial effects:
[0020] In the present application, graphene oxide significantly improves the catalytic effect of manganese dioxide on potassium permanganate, and the addition of graphene oxide and manganese dioxide can significantly improve the polishing effect of aluminum oxide abrasives on silicon carbide. The polishing rate of the prepared high catalytic activity manganese-based composite abrasives on silicon carbide is as high as 1000nm / h or more. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of a scanning electron microscope of the high catalytic activity manganese-based composite abrasive in Example 1. DETAILED DESCRIPTION
[0022] In order to make the objectives, technical solutions and advantages of the present invention more clear, the specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.
[0023] The present application provides a method for preparing a manganese-based composite abrasive with high catalytic activity, comprising:
[0024] S01: Add solid ice, concentrated sulfuric acid, graphite powder and sodium nitrate into a flask; wherein the mass ratio of concentrated sulfuric acid, graphite powder and sodium nitrate is 430:6:3.
[0025] S02: Stir the solution at 5°C, then add potassium permanganate; slowly drip deionized water, raise the temperature to 35°C and maintain for 2 hours; wherein the mass ratio of potassium permanganate to deionized water is 9:144.
[0026] S03: heating the mixed solution to 98°C and maintaining for 15 minutes;
[0027] S04: After the mixed solution is cooled to room temperature, a hydrogen peroxide solution is added to the mixed solution to obtain a bright yellow solution; wherein the concentration of the hydrogen peroxide solution is 30 wt.%, and the mass ratio of the hydrogen peroxide solution to the potassium permanganate in step S02 is 30:9.
[0028] S05: After washing the bright yellow solution with dilute hydrochloric acid, the separation method of suction filtration, centrifugation and drying is adopted to obtain graphene oxide; wherein the dilute hydrochloric acid is prepared by mixing concentrated hydrochloric acid and deionized water in a volume ratio, the concentration of the concentrated hydrochloric acid is 37wt.%, the volume ratio of concentrated hydrochloric acid and deionized water is 1:3, and the mass ratio of the dilute hydrochloric acid and the deionized water in S02 is 1:1.
[0029] S06: Graphene oxide is dispersed in deionized water by ultrasonic method, and potassium permanganate is added after adding manganese sulfate until the solution does not fade, so that manganese dioxide is precipitated on the graphene oxide; aluminum oxide abrasive is added and ultrasonically dispersed, so that the abrasive is impregnated on the graphene oxide to obtain manganese-based composite abrasive. The mass ratio of graphene oxide, manganese sulfate and aluminum oxide abrasive is 0.5:0.0521:1.
[0030] The present application provides a manganese-based composite abrasive with high catalytic activity, which is prepared by the preparation method described above. Graphene oxide significantly improves the catalytic effect of manganese dioxide on potassium permanganate, thereby improving the polishing rate.
[0031] The present application provides an application of a highly catalytically active manganese-based composite abrasive for preparing a polishing liquid for silicon carbide. The addition of graphene oxide and manganese dioxide can significantly improve the polishing effect of aluminum oxide abrasive on silicon carbide. The polishing rate of Example 1 reaches 1020nm / h, which means that graphene oxide significantly improves the catalytic effect of manganese dioxide on potassium permanganate, thereby improving the polishing rate.
[0032] Example 1
[0033] In this embodiment, a method for preparing a manganese-based composite abrasive with high catalytic activity is provided, wherein the raw materials include concentrated sulfuric acid, graphite powder, sodium nitrate, potassium permanganate, hydrogen peroxide solution, concentrated hydrochloric acid, manganese sulfate and aluminum oxide abrasive, wherein all the chemicals are of analytical purity.
[0034] The preparation method of the manganese-based composite abrasive with high catalytic activity is as follows:
[0035] (1) Under low temperature conditions using solid ice, add 144 ml of concentrated sulfuric acid, 3 g of graphite powder, and 1.5 g of sodium nitrate into a flask;
[0036] (2) stirring at 5° C. for half an hour, then slowly adding 9 g of potassium permanganate; then slowly dripping 144 ml of deionized water, raising the temperature to 35° C. and maintaining it for 2 hours to promote the oxidation reaction of graphite by potassium permanganate and concentrated sulfuric acid;
[0037] (3) Subsequently, the mixed solution was heated to 98°C and maintained for 15 minutes.
[0038] (4) After the mixed solution is cooled to room temperature, 30 ml of 30 wt.% hydrogen peroxide solution is poured into the mixed solution to remove the potassium permanganate that has not participated in the reaction. At this time, the solution turns bright yellow;
[0039] (5) washing the bright yellow solution with 300 ml of dilute hydrochloric acid (concentrated hydrochloric acid / deionized water = 1:10), and then obtaining graphene oxide by a separation method of suction filtration, high-speed centrifugation and drying;
[0040] (6) 0.5 g of graphene oxide was dispersed into 500 ml of deionized water by ultrasonication, and 0.0521 g of manganese sulfate was added, followed by slow dropwise addition of potassium permanganate until the potassium permanganate stopped fading, thereby 0.05 g of manganese dioxide was precipitated on the graphene oxide, and then 1 g of aluminum oxide abrasive was added to allow the abrasive to be impregnated on the graphene oxide, thereby obtaining manganese-based inorganic composite abrasive. The prepared manganese-based inorganic composite abrasive is as follows: Figure 1 shown.
[0041] (7) A polishing liquid was prepared using potassium permanganate as an oxidant and a highly catalytically active manganese-based composite abrasive as an abrasive, and a chemical mechanical polishing experiment was carried out on silicon carbide.
[0042] Comparative Example 1
[0043] In this embodiment, a method for preparing aluminum oxide composite abrasive grains is provided, wherein the raw materials for preparation include concentrated sulfuric acid, graphite powder, sodium nitrate, potassium permanganate, hydrogen peroxide solution, concentrated hydrochloric acid and aluminum oxide abrasive grains, wherein all the chemicals are of analytical purity.
[0044] The preparation method of the aluminum oxide composite abrasive is as follows:
[0045] (1) Under low temperature conditions using solid ice, add 144 ml of concentrated sulfuric acid, 3 g of graphite powder, and 1.5 g of sodium nitrate into a flask;
[0046] (2) stirring at 5° C. for half an hour, then slowly adding 9 g of potassium permanganate; then slowly dripping 144 ml of deionized water, raising the temperature to 35° C. and maintaining it for 2 hours to promote the oxidation reaction of graphite by potassium permanganate and concentrated sulfuric acid;
[0047] (3) Subsequently, the mixed solution was heated to 98°C and maintained for 15 minutes.
[0048] (4) After the mixed solution is cooled to room temperature, 30 ml of 30 wt.% hydrogen peroxide solution is poured into the mixed solution to remove the potassium permanganate that has not participated in the reaction. At this time, the solution turns bright yellow;
[0049] (5) washing the bright yellow solution with 300 ml of dilute hydrochloric acid (concentrated hydrochloric acid / deionized water = 1:10), and then obtaining graphene oxide by a separation method of suction filtration, high-speed centrifugation and drying;
[0050] (6) 0.5 g of graphene oxide was dispersed into 500 ml of deionized water by ultrasonic method, and then 1 g of aluminum oxide abrasive was added so that the abrasive was impregnated on the graphene oxide, and finally an aluminum oxide composite abrasive was obtained.
[0051] (7) A polishing liquid was prepared using potassium permanganate as an oxidant and an aluminum oxide composite abrasive as an abrasive, and a chemical mechanical polishing experiment was carried out on silicon carbide.
[0052] Comparative Example 2
[0053] In this embodiment, a method for preparing manganese-based composite abrasive is provided, wherein the preparation raw materials include potassium permanganate, manganese sulfate and aluminum oxide abrasive.
[0054] The preparation method of the manganese-based composite abrasive is as follows:
[0055] (1) 1 g of aluminum oxide abrasive was dispersed into 500 ml of deionized water by ultrasonic dispersion, and 0.0521 g of manganese sulfate was added followed by slow dropwise addition of potassium permanganate until the potassium permanganate stopped fading, thereby causing 0.05 g of manganese dioxide to precipitate on the aluminum oxide abrasive, thereby obtaining a manganese-based composite abrasive.
[0056] (2) A polishing liquid was prepared using potassium permanganate as an oxidant and manganese-based composite abrasives as abrasives, and a chemical mechanical polishing experiment was carried out on silicon carbide.
[0057] Performance Test:
[0058] 1. The mass of SiC wafer before and after polishing was measured by electronic balance (Mettler Toledo AG 285, accuracy: 0.01 mg), and the material removal rate of SiC wafer (nm / h) was calculated as follows: mass difference of SiC before and after polishing / (density of single crystal SiC × π* radius of wafer) 2 × polishing time).
[0059] Table 1 Performance test results
[0060] Sample source Material removal rate Example 1 1020nm / h Comparative Example 1 500nm / h Comparative Example 2 725nm / h
[0061] From the above performance test comparison, it can be seen that the addition of graphene oxide and manganese dioxide can significantly improve the polishing effect of aluminum oxide abrasives on silicon carbide. The polishing rate of Example 1 reached 1020nm / h, which means that graphene oxide significantly improves the catalytic effect of manganese dioxide on potassium permanganate, thereby improving the polishing rate.
[0062] The above description is only a preferred embodiment of the present invention, and the embodiment is not intended to limit the patent protection scope of the present invention. Therefore, all equivalent structural changes made using the description and drawings of the present invention should be included in the protection scope of the claims attached to the present invention.
Claims
1. A method for preparing a manganese-based composite abrasive with high catalytic activity, It is characterized in that include: S01: Add solid ice, concentrated sulfuric acid, graphite powder and sodium nitrate into a flask; S02: Stir the solution at 5°C, then add potassium permanganate; after adding deionized water, raise the temperature to 35°C and keep it for 2 hours; S03: heating the mixed solution to 98°C and maintaining for 15 minutes; S04: After the mixed solution is cooled to room temperature, a hydrogen peroxide solution is added to the mixed solution to obtain a bright yellow solution; S05: washing the bright yellow solution with dilute hydrochloric acid, and then obtaining graphene oxide by a separation method of suction filtration, centrifugation and drying; S06: dispersing graphene oxide into deionized water by ultrasonic means, adding manganese sulfate and then dropping potassium permanganate until the solution stops fading, so that manganese dioxide is precipitated on the graphene oxide; adding aluminum oxide abrasive and ultrasonically dispersing the abrasive so that the abrasive is impregnated on the graphene oxide, thereby obtaining manganese-based composite abrasive.
2. A method for preparing a manganese-based composite abrasive with high catalytic activity according to claim 1, It is characterized in that In step S01, the mass ratio of concentrated sulfuric acid, graphite powder and sodium nitrate is 430:6:
3.
3. A method for preparing a manganese-based composite abrasive with high catalytic activity according to claim 1, It is characterized in that In step S02, the mass ratio of potassium permanganate to deionized water is 9:
144.
4. The method for preparing a manganese-based composite abrasive with high catalytic activity according to claim 1, It is characterized in that The concentration of the hydrogen peroxide solution in step S04 is 30 wt.%, and the mass ratio of the hydrogen peroxide solution to the potassium permanganate in step S02 is 30:
9.
5. The method for preparing a manganese-based composite abrasive with high catalytic activity according to claim 1, It is characterized in that The dilute hydrochloric acid in step S05 is prepared by mixing concentrated hydrochloric acid and deionized water in a volume ratio, the concentration of the concentrated hydrochloric acid is 37wt.%, the volume ratio of concentrated hydrochloric acid to deionized water is 1:3, and the mass ratio of the dilute hydrochloric acid to the deionized water in S02 is 1:
1.
6. The method for preparing a manganese-based composite abrasive with high catalytic activity according to claim 1, It is characterized in that In step S06, the mass ratio of graphene oxide, manganese sulfate and aluminum oxide abrasive is 0.5:0.0521:
11.
7. A manganese-based composite abrasive with high catalytic activity, It is characterized in that The preparation method is described in any one of claims 1 to 6.
8. Use of a high catalytic activity manganese-based composite abrasive grain as claimed in claim 7, It is characterized in that Polishing fluid for preparing silicon carbide.