PH-stimulated slow-release type potassium humate water-retaining agent and synthesis method thereof
By combining solution polymerization method with potassium humate and sodium alginate, a pH-stimulated sustained release potassium humate water retention agent with biodegradability, sustained release and pH response sensitivity was prepared, and the existing technology was solved. The problems of poor biodegradability, improper water absorption rate and short nutrient release period have significantly improved fertilizer efficiency and water retention capabilities, and are suitable for crop growth in high-temperature and drought environments.
Patent Information
- Application Number
- CN202411063542.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-29
AI Technical Summary
Existing humic acid-based hydrogels have poor biodegradability, improper water absorption rate, short nutrient release period and low pH stimulation response sensitivity.
By combining components such as potassium humate, sodium alginate, sodium carboxymethylcellulose, acrylic acid, acrylamide and N,N'-methylenebisacrylamide, pH-stimulated sustained release humus is prepared by solution polymerization. Potassium water retention agent uses calcium chloride and potassium persulfate as curing agents and initiators to form a highly absorbent hydrogel with biodegradability, sustained release and pH response sensitivity.
A potassium humate water retention agent with both biodegradability, sustained release, pH response sensitivity and suitable water absorption ratio has been realized, which significantly improves fertilizer efficiency and reduces water evaporation and leakage. It is suitable for crops in high-temperature and arid environments. Grow.
Smart Images

Figure CN119039999A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water retaining agents, and particularly relates to a pH-stimulated slow-release potassium humate water retaining agent and a synthesis method thereof. Background Art
[0002] Potassium humate is a commonly used soil conditioner and natural organic potassium fertilizer, containing a large number of active functional groups (carboxyl, phenolic hydroxyl, etc.). Applying potassium humate water-soluble fertilizer can increase the content of soil organic matter and soil microorganisms on the one hand; on the other hand, it can promote the formation of soil aggregate structure and reduce the accumulation of salt in the surface soil; it can also increase the survival rate of plants and crops. However, in the natural environment of high temperature and drought, potassium humate aqueous solution will reduce fertilizer efficiency due to water loss in a short period of time, and too high concentration is not conducive to the growth and development of crops.
[0003] Potassium humate water retainer prepared with highly absorbent hydrogel as carrier can give full play to the fertilizer effect of potassium humate. Highly absorbent hydrogel is a kind of high molecular polymer with a three-dimensional cross-linked network structure and a large number of hydrophilic groups. When applied to the land, it can avoid water evaporation and leakage by absorbing irrigation water and rainwater. However, the humic acid hydrogels reported so far have problems such as poor biodegradability, improper water absorption rate, short nutrient release period and low pH stimulus response sensitivity. For example, the synthetic polymer hydrogel obtained by introducing potassium humate into the polymerization process of acrylic acid or acrylamide monomers takes several years to decades to degrade, but the natural hydrogel with good biodegradability usually has only a few dozen hours of nutrient release time due to its large number of hydrophilic functional groups; in addition, the reasonable water absorption multiple of the water retainer is preferably around 300 to 400 g / g. If it is too high, it will absorb water from plants, and if it is too low, the water storage capacity will be small. The water absorption multiple of sodium alginate-based potassium humate hydrogel is often as low as less than 100 g / g, and the water absorption multiple of acrylic acid hydrogel can exceed 1000 g / g. Therefore, it is of great significance to study a potassium humate water retainer that has both biodegradability, sustained release, pH response sensitivity and suitable water absorption multiple. Summary of the invention
[0004] In view of the problems in the prior art that humic acid-based hydrogels have poor biodegradability, too high or too low water absorption rate, short nutrient release period and low pH stimulation response sensitivity, the present invention provides a pH-stimulated sustained-release potassium humate water-retaining agent and a synthesis method thereof, thereby obtaining a potassium humate water-retaining agent having biodegradability, sustained-release properties, pH response sensitivity and suitable water absorption rate.
[0005] The present invention is achieved through the following technical solutions: A pH stimulated slow-release potassium humate water-retaining agent comprises the following ingredients in parts by weight: 0.3-0.5 parts of potassium humate, 1.5-3.0 parts of sodium alginate, 0.4-0.6 parts of sodium carboxymethyl cellulose, 7.5-22.5 parts of acrylic acid, 2.7-8.5 parts of alkali, 2.8-8.5 parts of acrylamide, 0.15-0.3 parts of N,N'-methylenebisacrylamide, 0.3-0.5 parts of curing agent, and 0.03-0.06 parts of initiator.
[0006] Furthermore, the alkali is sodium hydroxide or potassium hydroxide.
[0007] Furthermore, the curing agent is calcium chloride or calcium lactate.
[0008] Furthermore, the initiator is potassium persulfate, sodium persulfate or ammonium persulfate.
[0009] In the present invention, the synthesis method of the pH-stimulated slow-release potassium humate water-retaining agent comprises the following steps: (1) Add sodium alginate and sodium carboxymethyl cellulose to a 60-80 ℃ potassium humate aqueous solution and stir to dissolve; (2) The solution of step (1) is cooled to room temperature, acrylic acid is slowly added, stirred to dissolve, and alkali is added, stirred until dissolved; (3) Add acrylamide and N,N'-methylenebisacrylamide to the reaction solution of step (2) and dissolve them; (4) adding a mixed solution of a curing agent and an initiator to the dissolved solution in step (3), and stirring to obtain a mixed solution; (5) The mixed solution of step (4) is transferred to a mold, heated to 60-80°C, and kept warm for 1-2 h until the mixed solution solidifies.
[0010] (6) The mold containing the coagulation solution in step (5) is dried at room temperature for 8 to 24 hours to obtain a pH-stimulated slow-release potassium humate water-retaining agent.
[0011] Furthermore, the mass ratio of potassium humate to water in step (1) is 0.3-0.5:100.
[0012] Furthermore, the mass percentage concentration of the mixed solution of curing agent and initiator described in step (4) is 2-2.5%.
[0013] Furthermore, the mold in step (5) is a porous silicone mold.
[0014] Beneficial Effects The present invention uses potassium humate as filler, biodegradable sodium alginate and sodium carboxymethyl cellulose as matrix, N,N'-methylenebisacrylamide as crosslinking agent, and under the action of curing agent and initiator, two monomers of acrylamide and acrylic acid are grafted onto the sodium alginate / sodium carboxymethyl cellulose skeleton by solution polymerization to obtain a potassium humate water retainer with biodegradability, sustained release, pH response sensitivity and suitable water absorption rate. The potassium humate water retainer synthesized according to the present technology has biodegradability, pH stimulus responsiveness, sustained release and suitable water retention. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a photo of the appearance of pH-stimulated slow-release potassium humate water-retaining agent; Figure 2 This is the linear relationship fitting diagram between the concentration of potassium humate and absorbance measured by UV-visible absorption spectrum; Figure 3 These are pictures of pH-stimulated sustained-release potassium humate water-retaining agent under different pH conditions and after 72 hours.
[0016] Figure 4 This is a comparison chart of the leaf sizes of mulberry trees for fodder. Water retaining agent was applied to No. 1 to 5, but not to No. 6 to 10. DETAILED DESCRIPTION
[0017] The present invention is described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited by the embodiments. All technologies implemented based on the above content of the present invention are included in the scope of protection intended by the present invention.
[0018] Example 1 (1) Add 2.0 g sodium alginate and 0.5 g sodium carboxymethyl cellulose to a potassium humate aqueous solution (0.4 g potassium humate dissolved in 100 mL deionized water at 60 °C) and stir to dissolve. (2) The solution in step (1) was cooled to room temperature, 7.5 g of acrylic acid was slowly added, stirred for 5 min, and 2.7 g of solid sodium hydroxide was added, stirred for 10 min until it was evenly dissolved; (3) The reaction solution in step (2) was heated to room temperature (25°C), 2.82 g acrylamide and 0.15 g N,N'-methylenebisacrylamide were added, and stirred for 5 min until fully dissolved; (4) Add 20 mL of a pre-prepared mixed solution of calcium chloride and potassium persulfate (2.0% calcium chloride and 0.15% potassium persulfate) to the dissolved solution in step (3), and stir for 5 minutes to obtain a mixed solution; (5) The mixed solution of step (4) was allowed to stand for 5 min, added to the holes of the silica gel porous mold using a pipette, and placed in a 60°C oven for 1 h. The hydroxyl radicals generated by potassium persulfate will quickly initiate the graft polymerization of acrylic acid, acrylamide, sodium alginate, and sodium carboxymethyl cellulose.
[0019] (6) The mold containing the coagulation solution in step (5) is placed at room temperature and dried for 8 hours to obtain a pH-stimulated slow-release potassium humate water-retaining agent.
[0020] Example 2 (1) Add 2.0 g sodium alginate and 0.5 g sodium carboxymethyl cellulose to a potassium humate aqueous solution (0.4 g potassium humate dissolved in 100 mL deionized water at 80 °C) and stir to dissolve; (2) The solution in step (1) was cooled to room temperature, 15.1 g acrylic acid was slowly added, stirred for 5 min, and 5.4 g solid sodium hydroxide was added, stirred for 10 min until it was evenly dissolved; (3) The reaction solution in step (2) was heated to room temperature (25°C), 5.6 g acrylamide and 0.2 g N,N'-methylenebisacrylamide were added, and stirred for 5 min until fully dissolved; (4) Add 20 mL of a pre-prepared mixed solution of calcium chloride and potassium persulfate (2.0% calcium chloride and 0.2% potassium persulfate) to the dissolved solution in step (3), and stir for 5 minutes to obtain a mixed solution; (5) The mixed solution of step (4) was allowed to stand for 5 min, then added to the holes of the silica gel porous mold using a pipette, and placed in a 70°C oven for 1 h. The hydroxyl radicals generated by potassium persulfate will rapidly initiate the graft polymerization of acrylic acid, acrylamide, sodium alginate, and sodium carboxymethyl cellulose.
[0021] (6) The mold containing the coagulation solution in step (5) is placed at room temperature and dried for 16 hours to obtain a pH-stimulated slow-release potassium humate water-retaining agent.
[0022] Example 3 (1) Add 2.0 g sodium alginate and 0.5 g sodium carboxymethyl cellulose to a potassium humate aqueous solution (0.4 g potassium humate dissolved in 100 mL deionized water at 80 °C) and stir to dissolve; (2) The solution in step (1) was cooled to room temperature, 22.5 g of acrylic acid was slowly added, stirred for 5 min, and 8.5 g of solid sodium hydroxide was added, stirred for 10 min until it was evenly dissolved; (3) The reaction solution in step (2) was heated to room temperature (25°C), 8.5 g acrylamide and 0.3 g N,N'-methylenebisacrylamide were added, and stirred for 5 min until fully dissolved; (4) Add 20 mL of a pre-prepared mixed solution of calcium chloride and potassium persulfate (2.0% calcium chloride and 0.3% potassium persulfate) to the dissolved solution in step (3), and stir for 5 minutes to obtain a mixed solution; (5) The mixed solution of step (4) was allowed to stand for 5 min, added to the holes of the silica gel porous mold using a pipette, and placed in an oven at 80°C for 1 h. The hydroxyl radicals generated by potassium persulfate will quickly initiate the graft polymerization of acrylic acid, acrylamide, sodium alginate and sodium carboxymethyl cellulose.
[0023] (6) The mold containing the coagulation solution in step (5) is placed at room temperature and dried for 24 hours to obtain a pH-stimulated slow-release potassium humate water-retaining agent.
[0024] Performance Testing 1. The appearance photo of the pH-stimulated sustained-release potassium humate water-retaining agent prepared in Example 1 is as follows Figure 1 shown.
[0025] 2. Water absorption test (1) Accurately weigh two portions of pH-stimulated slow-release potassium humate water-retaining agent into a beaker (the initial weight is recorded as m 0) and immersed in 500 mL of distilled water respectively.
[0026] (2) At regular intervals, place the swollen water retaining agent on a 100-mesh sieve to filter out excess water, and weigh the swollen water retaining agent ( m 1).
[0027] (3) The calculation formula of water absorption multiple is as follows: Water absorption multiple (g / g) = ( m 1- m 0) / m 0 The water absorption multiples of the pH-stimulated sustained-release potassium humate water retaining agent prepared in Examples 1 to 3 within 2 days are shown in Table 1. As can be seen from Table 1, the water absorption multiples of the pH-stimulated sustained-release potassium humate water retaining agent prepared in Examples 1 to 3 after being immersed in distilled water for 2880 min are 330.7, 311.4, and 300.0 g / g, respectively, reaching the water absorption multiple range of the best water retaining agent (about 300 to 400 g / g).
[0028] Table 1 Water absorption test of pH-stimulated slow-release potassium humate water-retaining agent 3. Water loss rate test under natural air drying conditions (1) Soak the water retaining agent in 500 mL of distilled water for 48 hours; (2) After taking it out, filter the water with a 100-mesh sieve and weigh the weight of the water-retaining agent after swelling (w 0).
[0029] (3) Place it outdoors under natural light and air drying conditions for a certain period of time, and weigh it again ( w 1).
[0030] (4) The water loss rate of water retaining agent under natural air drying conditions is calculated as follows: Water loss rate (%) = ( w 0- w 1) / w 0×100% The pH-stimulated sustained-release potassium humate water-retaining agent prepared in Examples 1 to 3 was tested for its water loss rate under natural air-drying conditions as shown in Table 2. According to Table 2, the water loss rate of the pH-stimulated sustained-release potassium humate water-retaining agent prepared in Examples 1 to 3 was 80.1-92.2% after being placed under natural air-drying conditions for 38 h, and the water loss rate at the 72nd to 168th hour tended to be stable, which were 94.9%, 96.0%, and 98.1%, respectively.
[0031] Table 2 Water loss rate test table of pH stimulated slow-release potassium humate water retaining agent under natural air drying conditions 4. Soil water holding capacity test (1) Weigh the weight w 0 of saline-alkali soil in Linxi County, Chifeng, and then weighed 2% w 0 dry water retaining agent.
[0032] (2) Soak the water retaining agent in 500 mL of distilled water for 48 h, put it into a 150-mesh nylon net bag, and mix it with the soil.
[0033] (3) After a certain period of time, take out the net bag and weigh the soil again (mark w 1).
[0034] (4) The calculation formula of soil water holding capacity is as follows: Soil water holding capacity (%) = ( w 1- w 0) / w 0×100% The pH-stimulated slow-release potassium humate water retainer prepared in Examples 1 to 3, the soil water retention rate of the test soil after applying water retention for 168 hours is shown in Table 3 below. According to Table 3, as the soil contacts the water retainer for a longer time, the soil water retention rate shows an upward trend, eventually reaching 53.5%, 47.1%, and 41.3%, indicating that the prepared pH-stimulated slow-release potassium humate water retainer can provide moisture for plants and crops in the soil and reduce irrigation costs. In addition, it can be seen that compared with the water loss rate test results under natural air drying conditions, the pH-stimulated slow-release potassium humate water retainer prepared in Examples 1 to 3 is more helpful in maintaining soil moisture.
[0035] Table 3 Test table of the effect of pH-stimulated slow-release potassium humate water-retaining agent on soil water holding rate 5. pH stimulation effect test (1) Accurately weigh 1.0000 g of potassium humate black powder and dilute it to 1 L with distilled water in a volumetric flask. Take a certain volume to prepare potassium humate solutions with concentrations of 0.00013, 0.00038, 0.00063, 0.00100, 0.00125, 0.00188, and 0.00250 mol / L.
[0036] (2) Use an ultraviolet spectrophotometer to scan the prepared potassium humate solution and distilled water at a wavelength of 340 nm to obtain the following: Figure 2 The linear fitting equation shown is ( y = 327.96674 x + 0.01489).
[0037] (3) Weigh a certain amount of potassium dihydrogen phosphate, dipotassium hydrogen phosphate, hydrochloric acid and sodium hydroxide to prepare buffer solutions with simulated soil pH values of 5, 6, 7, 8, 9 and 10.
[0038] (4) Place 0.50 g of dry water retainer into 50 mL of buffer solution with different pH values. Use a syringe equipped with a 0.45 μm pore size polytetrafluoroethylene membrane filter to take 2 mL of sample for testing at regular intervals. Scan the absorbance of the sample at a wavelength of 340 nm, and calculate the concentration of released potassium humate based on the fitting equation.
[0039] The pH-stimulated slow-release potassium humate water-retaining agent prepared in Examples 1 to 3 was placed in a buffer solution (made of potassium dihydrogen phosphate, dipotassium hydrogen phosphate, hydrochloric acid, and sodium hydroxide). The images of the pH-stimulated slow-release potassium humate water-retaining agent after 72 hours under different pH conditions are shown in the following figure. Figure 3As shown. The release rates of potassium humate at different pH and soaking time are shown in Table 4. As can be seen from Table 4, the release rates of potassium humate of the pH-stimulated sustained-release potassium humate water-retaining agent prepared in Example 1 at 500 h (about 21 days) were 22.53%, 27.07%, 30.65%, 35.72%, 41.51%, and 54.21%, respectively, which have obvious sustained-release effects. Moreover, with the increase of the pH value of the buffer solution and the soaking time, the release rate of potassium humate shows a trend of increasing, which may be related to the presence of a large number of carboxyl groups in the molecules of sodium alginate and sodium carboxymethyl cellulose. In an alkaline environment, the carboxyl groups are deprotonated, the electrostatic repulsion increases, and the gel network becomes loose, which is conducive to the release of potassium humate.
[0040] In addition, as shown in Tables 5 and 6, with the increase in the weight ratio of acrylic acid and acrylamide added during the synthesis of Example 2 and Example 3, the release rate of potassium humate becomes 16.79%, 23.35%, 27.27%, 36.92%, 43.87%, 53.78% and 11.00%, 19.61%, 23.91%, 38.14%, 46.24%, 55.30%, that is, a more obvious difference in release rate is shown at lower pH (5, 6, 7), which reflects that the pH-stimulated sustained-release potassium humate water-retaining agent prepared in Example 2 and Example 3 has a better pH response sensitivity. This result may be attributed to the increase in the amount of acrylic acid input during the synthesis process, which increases the number of carboxyl functional groups in the hydrogel. In an acidic environment, these carboxyl groups tend to be protonated, resulting in a decrease in the electrostatic repulsion between molecules and a tighter gel network structure, thereby limiting the release of potassium humate.
[0041] Table 4 Release rate of pH-stimulated sustained-release potassium humate water-retaining agent in Example 1 in buffer solutions with different pH values Table 5 Release rate of pH-stimulated sustained-release potassium humate water-retaining agent in Example 2 in buffer solutions with different pH values Table 6 Release rate of pH-stimulated sustained-release potassium humate water-retaining agent in Example 3 in buffer solutions with different pH values 6. Statistics on the effects of water retaining agents on crop growth (1) Select a field with medium fertility in Quantai Village, Jinshan Town, Kalaqin Banner, Chifeng, divide it into two pieces, and dig out the soil in the middle (separated by about 5 cm) to reduce the interference between the two pieces of soil; (2) Keep the planting density and spacing of seedlings consistent, and plant mulberry seedlings of similar plant height and mesh size in the two plots. The left side is recorded as the blank control group, and the right side is recorded as the implementation group; (3) Considering that Example 1 has a higher water absorption multiple and potassium humate release rate than Examples 2 and 3, the pH-stimulated slow-release potassium humate water-retaining agent prepared in Example 1 was applied to the soil around the seedlings on the right side at a dosage of 10 g / plant. During the entire test period, only conventional field care methods and natural rainfall were relied upon; (4) Record the plant height and the length of four leaves of each mulberry seedling at 15 days of growth, and calculate the average value; The pH-stimulated slow-release potassium humate water retainer prepared in Example 1 was tested for its effect on the plant height and leaf length of crops. The results are shown in Table 7. The leaf size of mulberry forage is Figure 4 Compare the data in Table 7 and Figure 4 From the displayed leaf sizes of fodder mulberry, it can be seen that the average plant height and average leaf length of fodder mulberry treated with pH-stimulated slow-release potassium humate water-retaining agent are greater, which has a significant fertilizer effect.
[0042] Table 7 Statistical table of the effect of pH-stimulated slow-release potassium humate water retaining agent on the growth of mulberry seedlings .
Claims
1. A pH-stimulated slow-release potassium humate water-retaining agent, characterized in that: The invention comprises the following ingredients in parts by weight: 0.3-0.5 parts of potassium humate, 1.5-3.0 parts of sodium alginate, 0.4-0.6 parts of sodium carboxymethyl cellulose, 7.5-22.5 parts of acrylic acid, 2.7-8.5 parts of alkali, 2.8-8.5 parts of acrylamide, 0.15-0.3 parts of N,N'-methylenebisacrylamide, 0.3-0.5 parts of curing agent and 0.03-0.06 parts of initiator.
2. The pH-stimulated sustained-release potassium humate water-retaining agent according to claim 1, characterized in that: The alkali is sodium hydroxide or potassium hydroxide.
3. The pH-stimulated sustained-release potassium humate water-retaining agent according to claim 1, characterized in that: The curing agent is calcium chloride or calcium lactate.
4. The pH-stimulated sustained-release potassium humate water-retaining agent according to claim 1, characterized in that: The initiator is potassium persulfate, sodium persulfate or ammonium persulfate.
5. A method for synthesizing the pH-stimulated sustained-release potassium humate water-retaining agent according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Add sodium alginate and sodium carboxymethyl cellulose to a 60-80 ℃ potassium humate aqueous solution and stir to dissolve; (2) The solution of step (1) is cooled to room temperature, acrylic acid is slowly added, stirred to dissolve, and alkali is added, stirred until dissolved; (3) Add acrylamide and N,N'-methylenebisacrylamide to the reaction solution of step (2) and dissolve them; (4) adding a mixed solution of a curing agent and an initiator to the dissolved solution in step (3), and stirring to obtain a mixed solution; (5) The mixed solution of step (4) is transferred to a mold, heated to 60-80°C, and kept warm for 1-2 h until the mixed solution solidifies. (6) The mold containing the coagulation solution in step (5) is dried at room temperature for 8 to 24 hours to obtain a pH-stimulated slow-release potassium humate water-retaining agent.
6. The method for synthesizing the pH-stimulated sustained-release potassium humate water-retaining agent according to claim 5, characterized in that: The mass ratio of potassium humate to water in step (1) is 0.3-0.5:
100.
7. The method for synthesizing the pH-stimulated sustained-release potassium humate water-retaining agent according to claim 5, characterized in that: The mass percentage concentration of the mixed solution of curing agent and initiator described in step (4) is 2-2.5%.
8. The method for synthesizing the pH-stimulated sustained-release potassium humate water-retaining agent according to claim 5, characterized in that: The mold in step (5) is a silicone porous mold.
Citation Information
Cited By
Water-retaining agent with salt resistance and urease inhibition effects as well as preparation method and application of water-retaining agent
CN120818367A