Maintenance method for bleed-out burn-through part of converter body

Through the laser thickness gauge measuring and combining internal patching and external spraying of chromium corundum mud, the problem of difficult and poor maintenance of steel leakage in the converter body is solved, and efficient gap filling and welding is achieved, which significantly improves maintenance Mass and furnace life.

CN119040551AActive Publication Date: 2024-11-29МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411108015.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-29
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The burn-through accident of the converter furnace body leakage steel is difficult, time-consuming and poor in maintenance. The existing technology cannot ensure the enrichment of magnesium-carbon brick gaps and the quality of sintering of the material.

Method used

Use laser thickness gauge to measure the residual thickness of the burned-through part of the furnace body leakage steel, combine internal magnesium carbon bricks and magnesium calcium spraying and wet spraying, chromium corundum mud spraying and welding to ensure gap filling and welding quality .

Benefits of technology

It improves maintenance quality, reduces the chance of steel leakage burning through again, reduces the labor intensity and maintenance costs of operators, and significantly increases the service life of the converter furnace body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040551A_ABST
    Figure CN119040551A_ABST
Patent Text Reader

Abstract

According to the maintenance method for the breakout burnthrough part of the converter body, corresponding molten steel and slag turning-over shutdown operation is adopted according to different breakout burnthrough parts of the converter body, and the situation that the breakout burnthrough parts of the converter body are damaged and aggravated is effectively avoided. And a laser thickness gauge is adopted to measure the residual thickness of the furnace lining brick at the breakout burnthrough part of the furnace body so as to determine the use amount of magnesia carbon bricks for maintenance and the specific maintenance position. According to the fact that the breakout burnthrough part of the converter body is not used, corresponding maintenance means are adopted in a targeted mode, namely, the mode of'sticking of magnesia carbon bricks and wet gunning of magnesia-calcium gunning materials' is adopted inside, the mode of'spraying of chrome corundum slurry and furnace shell welding repair 'is adopted outside, the breakout burnthrough part of the converter body is maintained by combining inside and outside, and the maintenance quality of the breakout burnthrough part can be effectively improved. Compared with a traditional maintenance mode, the probability of steel breakout and burnthrough of the steel breakout and burnthrough part of the converter body again is reduced to zero. The method is convenient to operate, time-saving and labor-saving, and has popularization and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of converter steelmaking furnace condition maintenance technology, and in particular relates to a method for maintaining a steel leakage burn-through portion of a converter furnace body. Background Art

[0002] The converter body is generally composed of a steel structure shell and a lining of refractory materials. The converter shell is welded from ordinary boiler steel plates or low-alloy steel plates. It can be divided into three parts: furnace cap, furnace body and furnace bottom according to different parts. Its function is to bear the total weight of refractory materials, molten steel and slag, and to keep the furnace in a fixed shape, and to withstand torsional torque when tilting; the converter lining refractory materials are mainly composed of an insulating layer, a permanent layer and a working layer.

[0003] In the actual smelting process, due to the extremely complex and intense physical and chemical reactions and mechanical movements in the converter, the converter lining is susceptible to erosion and damage during use, especially the superposition of adverse factors such as high temperature peroxidation, which will cause greater erosion to the lining. In serious cases, the converter body may even leak steel and burn through, which will cause huge hidden dangers to the safe production of the converter. Therefore, the service life of the converter lining has a very important impact on improving production efficiency, increasing furnace life, improving molten steel quality, improving variety structure, reducing refractory consumption, and increasing economic benefits. Due to the installation method of the furnace body and the support ring, as well as the heavy weight, it is very difficult to disassemble. Therefore, when the converter body leaks steel and burns through, it is very important to minimize the converter downtime and resume production.

[0004] The patent with publication number CN 110653450 A published on January 7, 2020 discloses an online repair method for perforation of a converter body, and the repair steps are: first, a working platform needs to be built on one side of the perforation of the furnace body; then, magnesia-carbon bricks for furnace building are inserted into the perforated position of the converter shell, and the perforated position of the converter shell is filled with magnesia-carbon bricks. The edge gaps of the magnesia-carbon bricks are filled, compacted, and fixed with mixed fire mud; then, repair welding is performed; finally, after the welding process is completed, the furnace is shaken to a position suitable for repairing the furnace, and the erosion pits of the furnace lining at the perforated position of the furnace shell are treated again, and the pits of the furnace lining are filled by sticking magnesia-carbon bricks and covering with hand-thrown furnace charge. This method has played a certain positive effect in the repair of perforation in the converter body, but this method requires the construction of a working platform. The operator on the working platform must first fill the perforation position with magnesia carbon bricks, and fill the edge gaps of the magnesia carbon bricks with fire mud, but it cannot ensure that the gaps between the magnesia carbon bricks are full, affecting the repair effect; in addition, when this method is used to treat the lining erosion pits at the perforation position of the furnace shell, due to the influence of the perforation position of the converter body, the method of pasting magnesia carbon bricks and covering with hand-thrown furnace charge cannot ensure that the hand-thrown charge can accurately cover the perforation position, and as the furnace temperature drops, the sintering quality of the refractory material also decreases, which also affects its repair effect to a certain extent. Summary of the invention

[0005] The purpose of the present invention is to provide a method for maintaining the steel leakage burn-through part of the converter body, which can effectively maintain the steel leakage burn-through part of the converter body, improve the service life of the converter lining, and reduce the labor intensity of operators. It solves the technical problems of difficulty, time-consuming and poor maintenance effect of the steel leakage burn-through part of the converter body.

[0006] The specific technical solutions of the present invention are as follows:

[0007] A method for maintaining a burn-through portion of a converter body having steel leakage comprises the following steps:

[0008] 1) When the converter body leaks and burns through, empty the molten steel and slag in the converter and shut down the furnace;

[0009] 2) Measure the residual thickness and damaged position of the furnace lining bricks at the leaky and burnt-through parts of the converter body, and determine the amount of maintenance materials and the specific maintenance location;

[0010] 3) First, maintain and sinter the damaged lining of the converter body where steel leaks and burns through;

[0011] 4) Mix the chrome corundum castable with water to make chrome corundum slurry, and spray the chrome corundum slurry into the steel leakage and burn-through parts of the converter body from the external furnace shell to fill and compact the gap between the furnace shell steel plate and the furnace lining for sintering;

[0012] 5) Finally, the furnace shell of the converter body where steel has leaked and burned through is repaired by welding.

[0013] In step 1), when the converter body steel leakage and burn-through accident occurs, according to the different parts of the converter body steel leakage and burn-through, select the corresponding treatment method to empty the molten steel and slag in the converter in time to prevent the accident from expanding and create conditions for the next step of the furnace body steel leakage and burn-through maintenance, as follows:

[0014] 1-1) When the accident of steel leakage and burning through of the furnace body on the slag pouring side of the converter occurs, the converter is tilted toward the steel tapping side, and the molten steel and slag in the furnace are poured into the ladle from the furnace mouth and emptied to prevent the steel structure of the furnace shell from being further burned at the part where the furnace body on the slag pouring side of the converter is burned through.

[0015] 1-2) When the accident of steel leakage and burning through of the furnace body on the steel-tapping side of the converter occurs, the converter is tilted to the slag-discharging side, and the molten steel and slag in the furnace are poured into the ladle from the furnace mouth and emptied to prevent the steel structure of the furnace shell from being further burned out at the burn-through part of the furnace body on the steel-tapping side of the converter.

[0016] 1-3) When the accident of steel leakage and burning through of the converter ear shaft area occurs, the converter is tilted to the slag discharge side or the steel tapping side, and the molten steel and slag in the furnace are poured into the ladle from the furnace mouth and emptied to prevent the steel structure of the furnace shell from being further burned out at the burn-through part of the converter ear shaft area.

[0017] 1-4) When a steel leakage and burn-through accident occurs in the cap area on the slag pouring side of the converter, the converter is tilted toward the steel tapping side to pour the molten steel and slag in the furnace into the ladle from the furnace mouth and then empty it to prevent the steel structure of the furnace shell from being further burned in the cap area on the slag pouring side of the converter.

[0018] 1-5) When a steel leakage and burn-through accident occurs in the cap area on the steel-out side of the converter, the converter is tilted toward the slag discharge side to pour the molten steel and slag in the furnace into the ladle from the furnace mouth and then empty it to prevent the steel structure of the furnace shell from being burned through in the cap area on the steel-out side of the converter from being further burned.

[0019] 1-6) When a steel leakage or burn-through accident occurs in the converter bottom area, the converter is tilted toward the slag discharge side or the steel tapping side to pour the molten steel and slag in the furnace into the ladle from the furnace mouth and empty it to prevent further burning of the furnace shell steel structure at the converter bottom area where the furnace body is burned through.

[0020] In step 2), after the molten steel and slag in the converter are emptied, a laser thickness gauge is used to measure the residual thickness and damaged position of the lining bricks at the leaking and burning parts of the converter body to determine the amount of magnesia carbon bricks used for maintenance and the specific maintenance position.

[0021] Preferably, when using magnesia carbon bricks, the reference amount of magnesia carbon bricks is appropriate to fill the depressions in the damaged furnace lining in the furnace, and is determined by the empirical formula:

[0022]

[0023] In formula (1), m is the amount of magnesia carbon bricks, the calculated result needs to be rounded and is a multiple of the weight of a single magnesia carbon brick, kg; M is the standard value of the new furnace lining thickness, which is 650 mm, mm; N is the residual thickness of the furnace lining bricks at the furnace body leakage and burn-through position, mm; 50 is the thickness of the magnesia carbon bricks, mm; 20 is the weight of a single magnesia carbon brick, kg.

[0024] Further, in step 2), the maintenance materials include magnesia carbon bricks, converter sand, magnesia calcium gunning material and chrome corundum castable;

[0025] The magnesia carbon brick is a 200mm×100mm×50mm rectangular block, with a single block weight of 20kg, w(MgO)≥72.00%, w(C 固 )≥18.00%;

[0026] The converter sand is in granular form, with a particle size of ≤20 mm, w(MgO)≥78.00%, w(C 固 )≥2.50%;

[0027] The magnesium-calcium gunning material is in the form of particles, with a particle size of ≤3.00 mm, w(MgO)≥80.00%, w(CaO≥7.00%, w(SiO2)≤5.00%, and w(H2O≤0.50%;

[0028] The chrome corundum casting material is in the form of fine-grained powder, with a particle size of ≤0.20 mm, w(Al2O3)≥85.00%, w(Cr2O3)≥5.00%, and w(Fe2O3)≤1.50%.

[0029] The technical indicators of magnesia carbon bricks are: volume density ≥ 2.90g / cm 3 , compressive strength ≥35.00MPa, apparent porosity ≤3.00%, high temperature flexural strength ≥10.00MPa in reducing atmosphere 1400℃×0.5h;

[0030] The technical indicators of magnesium-calcium gunning materials are: refractoriness ≥1760℃; under the condition of 110℃×24h: volume density ≥2.20g / cm 3 , compressive strength ≥7.00MPa; under the condition of 1500℃×3h: compressive strength ≥15.00MPa, flexural strength ≥5.00MPa, linear change rate -2.5~0%;

[0031] The technical indicators of chrome corundum castables are: refractoriness ≥1780℃; under the condition of 110℃×24h: volume density ≥3.00g / cm 3 , compressive strength ≥50.00MPa, flexural strength ≥10.00MPa; under the conditions of 1500℃×3h: compressive strength ≥80.00, flexural strength ≥25.00MPa, linear change rate -0.30~0%;

[0032] In step 3), the damaged lining of the converter body where steel leaks and burns through is first maintained from the inside, specifically:

[0033] When leakage and burning through occur in the furnace body on the slag pouring side, the furnace body on the steel tapping side, the furnace body in the trunnion area of ​​the converter, the furnace cap area on the slag pouring side of the converter and the furnace cap area on the steel tapping side of the converter, firstly use magnesia carbon bricks to maintain the damaged lining position in the furnace, and then use magnesia calcium gunning material mixed with water to gunning to fill the gaps between the magnesia carbon bricks after gunning, and then sinter, the sintering temperature is ≥1620℃, and the sintering time is 20-25min; the weight ratio of the magnesia calcium gunning material to water is 1:1.0-1:1.3;

[0034] In step 3), the gunning pressure is controlled at 0.3-0.5 MPa;

[0035] When steel leakage and burn-through occur in the bottom area of ​​the converter, add converter sand into the furnace from the converter mouth, and then shake the converter to an angle of 30°~40° towards the back and front of the furnace based on the zero position (vertical state). Shake the furnace repeatedly 2~3 times to ensure that the converter sand is completely spread and covers the damaged lining of the converter bottom where steel leakage and burn-through occur, and then sintering is carried out. The sintering temperature is ≥1620℃, and the sintering time is controlled at 50~60min.

[0036] In step 4), the mass ratio of chrome corundum castable to water is 1:0.30 to 1:0.35;

[0037] In step 4), the sintering temperature is 280-400° C. and the sintering time is 30-40 min;

[0038] In step 4), the pressure of the chrome corundum slurry injection is controlled at 0.2-0.4 MPa.

[0039] In step 5), the furnace shell of the converter where steel is leaking and burned through is repaired by welding using a steel plate made of the same material as the furnace shell.

[0040] Compared with the prior art, the present invention adopts corresponding molten steel and slag emptying and stopping operation according to the different parts of the furnace body where the steel leaks and burns through, which effectively avoids the aggravation of the damage to the parts where the steel leaks and burns through. A laser thickness gauge is used to measure the residual thickness of the furnace lining bricks at the parts where the steel leaks and burns through the furnace body, so as to determine the amount of magnesia carbon bricks used for maintenance and the specific maintenance position, provide a scientific basis for the precise implementation of maintenance at this location, avoid the waste of maintenance refractory materials, and reduce maintenance costs. According to the parts where the steel leaks and burns through the converter body, corresponding maintenance measures are taken in a targeted manner, that is, the internal "patching magnesia carbon bricks + magnesia calcium gunning material wet gunning" method is adopted, and the external "spraying chrome corundum mud + furnace shell welding" method is adopted. The internal and external combined maintenance of the parts where the steel leaks and burns through the converter body can effectively improve the maintenance quality of the parts. And the method of spraying chrome corundum mud has fluidity, which is conducive to filling and compacting the gap between the furnace shell and the furnace lining bricks. Compared with the traditional maintenance method, the probability of steel leaking and burning through again at the parts where the steel leaks and burns through the converter body is reduced to zero. The method of the invention is easy to operate, saves time and effort, and has good promotion and application prospects in the maintenance of steel leakage and burn-through parts of converter furnace bodies in similar steel enterprises. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a schematic diagram of the operating process of the maintenance method for the steel leakage and burn-through parts of the converter furnace body. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] The present invention provides a method for maintaining a burn-through portion of a converter body, comprising the following steps:

[0044] 1) Turn over and stop the furnace:

[0045] When a converter body leaks and burns through an accident, according to the different locations of the converter body leaking and burning through, select the appropriate treatment method to empty the molten steel and slag in the converter in time to prevent the accident from expanding and create conditions for the next step of maintenance of the furnace body leaking and burning through. The details are as follows:

[0046] 1-1) When the accident of steel leakage and burning through of the furnace body on the slag pouring side of the converter occurs, the converter is tilted toward the steel tapping side, and the molten steel and slag in the furnace are poured into the ladle from the furnace mouth and emptied to prevent the steel structure of the furnace shell from being further burned at the part where the furnace body on the slag pouring side of the converter is burned through.

[0047] 1-2) When the accident of steel leakage and burning through of the furnace body on the steel-tapping side of the converter occurs, the converter is tilted to the slag-discharging side, and the molten steel and slag in the furnace are poured into the ladle from the furnace mouth and emptied to prevent the steel structure of the furnace shell from being further burned out at the burn-through part of the furnace body on the steel-tapping side of the converter.

[0048] 1-3) When the accident of steel leakage and burning through of the converter ear shaft area occurs, the converter is tilted to the slag discharge side or the steel tapping side, and the molten steel and slag in the furnace are poured into the ladle from the furnace mouth and emptied to prevent the steel structure of the furnace shell from being further burned out at the burn-through part of the converter ear shaft area.

[0049] 1-4) When a steel leakage and burn-through accident occurs in the cap area on the slag pouring side of the converter, the converter is tilted toward the steel tapping side to pour the molten steel and slag in the furnace into the ladle from the furnace mouth and then empty it to prevent the steel structure of the furnace shell from being further burned in the cap area on the slag pouring side of the converter.

[0050] 1-5) When a steel leakage and burn-through accident occurs in the cap area on the steel-out side of the converter, the converter is tilted toward the slag discharge side to pour the molten steel and slag in the furnace into the ladle from the furnace mouth and then empty it to prevent the steel structure of the furnace shell from being burned through in the cap area on the steel-out side of the converter from being further burned.

[0051] 1-6) When a steel leakage or burn-through accident occurs in the converter bottom area, the converter is tilted toward the slag discharge side or the steel tapping side to pour the molten steel and slag in the furnace into the ladle from the furnace mouth and empty it to prevent further burning of the furnace shell steel structure at the converter bottom area where the furnace body is burned through.

[0052] 2) Maintenance refractory preparation:

[0053] The refractory materials used for the maintenance of the steel leakage and burn-through parts of the converter body mainly include magnesia carbon bricks, converter sand, magnesia calcium gunning materials and chrome corundum castables. Among them, magnesia carbon bricks are 200mm×100mm×50mm rectangular blocks, with a single block weight of 20kg, w(MgO)≥72.00%, w(C 固 )≥18.00%; converter sand is in granular form, with a particle size of ≤20mm, w(MgO)≥78.00%, w(C 固)≥2.50%; magnesium-calcium gunning material is in granular form, with a particle size of ≤3.00mm, w(MgO)≥80.00%, w(CaO)≥7.00%, w(SiO2)≤5.00%, w(H2O)≤0.50%; chrome corundum castable is in fine granular powder form, with a particle size of ≤0.20mm, w(Al2O3)≥85.00%, w(Cr2O3)≥5.00%, w(Fe2O3)≤1.50%. The technical indicators of magnesium-carbon bricks, magnesium-calcium gunning material and chrome corundum castable are shown in Table 1, Table 2 and Table 3 respectively.

[0054] Table 1 Technical indicators of magnesia carbon bricks

[0055]

[0056] Table 2 Technical indicators of magnesium calcium gunning materials

[0057]

[0058] Table 3 Technical indicators of chrome corundum castables

[0059]

[0060] 3) Thickness measurement and positioning

[0061] After the molten steel and slag in the converter are emptied, the Lacam M3 laser thickness gauge is used to measure the residual thickness and damaged position of the lining bricks at the leaking and burning parts of the converter body to determine the amount of magnesia carbon bricks used for maintenance and the specific maintenance position. Among them, the reference amount of magnesia carbon bricks is preferably used to fill the concave parts of the damaged lining in the furnace, and is determined by the empirical formula:

[0062]

[0063] In formula (1), m is the amount of magnesia carbon bricks, the calculated result needs to be rounded and is a multiple of the weight of a single magnesia carbon brick, kg; M is the standard value of the new furnace lining thickness (this value is 650mm), mm; N is the residual thickness of the furnace lining bricks at the furnace body leakage and burn-through position, mm; 50 is the thickness of the magnesia carbon bricks, mm; 20 is the weight of a single magnesia carbon brick, kg.

[0064] 4) Maintenance operation process

[0065] According to the measurement results of the Lacam M3 laser thickness gauge, the converter body leaking and burnt-through parts are maintained in the order of "internal repair first and external repair later" and the principle of "high-temperature hot repair", that is, first, the high temperature conditions in the furnace are beneficial to the sintering of refractory materials, and the "patching magnesia-carbon bricks + magnesium-calcium gunning material wet gunning repair" method is used to maintain the damaged lining of the converter body leaking and burnt-through parts from the inside, after sintering is completed; then, a concrete spraying machine is used to mix the chrome corundum castable with water to form a slurry, and the chrome corundum slurry is sprayed into the converter body leaking and burnt-through parts from the external furnace shell to fill and compact the gap between the furnace shell steel plate and the furnace lining, after sintering is completed; finally, the furnace shell of the converter body leaking and burnt-through parts is welded with a steel plate of the same material as the furnace shell. The specific operation procedures for different leaking and burnt-through parts are as follows:

[0066] 4-1) Maintenance of the steel leakage and burn-through parts of the converter slag pouring side:

[0067] 4-1-1) The converter is tilted to -90°~-100° toward the platform in front of the furnace, and the magnesia carbon bricks are delivered from the furnace mouth to the damaged lining position in the furnace by using a furnace repair shovel for brick laying maintenance. The aforementioned brick laying maintenance operation is repeated until the damaged lining at the furnace body leakage and burn-through position on the slag pouring side of the converter is filled.

[0068] 4-1-2) After the tile maintenance work is completed, the wet gunning process is used, and the compressed air pressure of the PB-II gunning tank is controlled at 0.3~0.5MPa. The magnesium calcium gunning material is mixed with water at a weight ratio of 1:1.0~1:1.3. After mixing through the gunning gun, the magnesium calcium gunning material is evenly and completely covered with the magnesium carbon bricks. The purpose is to fill the gaps between the magnesium carbon bricks after the patching, and improve the density and thermal shock resistance of the magnesium carbon after sintering. After the gunning operation is completed, the sintering temperature is ≥1620℃, and the sintering time is controlled at 20~25min.

[0069] 4-1-3) After the magnesium-calcium gunning material is fully sintered, the converter is shaken to the operating platform behind the furnace to 140°~150°, the compressed air pressure of the Xuda brand PZ-3 refractory material spraying machine is controlled at 0.2~0.4MPa, the chrome corundum castable and water are mixed at a weight ratio of 1:0.30~1:0.35, and the chrome corundum mud is obtained by mixing through the spray gun. The chrome corundum mud is sprayed from the outside of the furnace shell into the steel leakage and burnt-through parts of the furnace body on the slag pouring side of the converter to fill and compact the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 280~400℃, and the sintering time is controlled at 30~40min.

[0070] 4-1-4) After the chrome corundum slurry is fully sintered, the converter is then swung to the rear platform at 140°~150°, a maintenance work platform is built, and the furnace shell on the slag pouring side of the converter where steel is leaking and burned through is repaired by welding using steel plates of the same material as the furnace shell.

[0071] 4-2) Maintenance of the steel leakage and burn-through parts of the converter body on the steel tapping side

[0072] 4-2-1) The converter is tilted to 90°~100° toward the rear platform, and the magnesia carbon bricks are delivered from the furnace mouth to the damaged lining position in the furnace using a furnace repair shovel for brick laying maintenance. Repeat the aforementioned brick laying maintenance operation until the damaged lining at the furnace body on the steel-out side of the converter is filled.

[0073] 4-2-2) After the tile maintenance work is completed, the wet gunning process is used, and the compressed air pressure of the PB-II gunning tank is controlled at 0.3~0.5MPa. The magnesium calcium gunning material and water are mixed at a weight ratio of 1:1.0~1:1.3 through the gunning gun, and the magnesium calcium gunning material is evenly and completely covered with the magnesium carbon bricks. The purpose is to fill the gaps between the magnesium carbon bricks after the patching, and improve the density and thermal shock resistance of the magnesium carbon after sintering. After the gunning operation is completed, the sintering temperature is ≥1620℃, and the sintering time is controlled at 20~25min.

[0074] 4-2-3) After the magnesium-calcium gunning material is fully sintered, the converter is shaken to the platform in front of the furnace to -140°~-150°, and the compressed air pressure of the Xuda brand PZ-3 refractory material spraying machine is controlled at 0.2~0.4MPa. The chrome corundum castable and water are mixed in a weight ratio of 1:0.30~1:0.35 through a spray gun. The obtained chrome corundum slurry is sprayed from the outside of the furnace shell into the steel-outgoing side of the converter body where steel is leaking and burned through, filling and compacting the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 280~400℃, and the sintering time is controlled at 30~40min.

[0075] 4-2-4) After the chrome corundum slurry is fully sintered, the converter is shaken to the platform in front of the furnace to -140°~-150°, a maintenance work platform is built, and the furnace shell of the converter on the steel-out side where the furnace body is leaking and burned through is welded using steel plates of the same material as the furnace shell.

[0076] 4-3) Maintenance of the burn-through area of ​​the converter body in the trunnion area

[0077] 4-3-1) Swing the converter to 90°~100° toward the rear platform or -90°~-100° toward the front platform, use a furnace repair shovel to deliver magnesia carbon bricks from the furnace mouth to the damaged lining position in the furnace for brick laying maintenance, repeat the above-mentioned brick laying maintenance operation until the damaged lining at the converter ear shaft area where the furnace body has leaked and burned through is filled.

[0078] 4-3-2) After the tile maintenance work is completed, the wet gunning process is used, and the compressed air pressure of the PB-II gunning tank is controlled at 0.3~0.5MPa. The magnesium calcium gunning material and water are mixed at a weight ratio of 1:1.0~1:1.3 through the gunning gun, and the magnesium calcium gunning material is evenly and completely covered with the magnesium carbon bricks. The purpose is to fill the gaps between the magnesium carbon bricks after the patching, and improve the density and thermal shock resistance of the magnesium carbon after sintering. After the gunning operation is completed, the sintering temperature is ≥1620℃, and the sintering time is controlled at 20~25min.

[0079] 4-3-3) After the magnesium-calcium gunning material is fully sintered, the converter is shaken to 90°~100° behind the furnace or to -90°~-100° towards the platform in front of the furnace, and the compressed air pressure of the Xuda brand PZ-3 refractory material spraying machine is controlled at 0.2~0.4MPa. The chrome corundum castable and water are mixed in a weight ratio of 1:0.30~1:0.35 through a spray gun. The obtained chrome corundum slurry is sprayed from the outside of the furnace shell into the steel leakage and burnt-through parts of the furnace body in the ear shaft area of ​​the converter to fill and compact the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 280~400℃, and the sintering time is controlled at 30~40min.

[0080] 4-3-4) After the chrome corundum slurry is fully sintered, the converter is then moved to the rear platform to 90°~100° or the front platform to -90°~-100°, and a maintenance work platform is built. The furnace shell of the converter ear shaft area where steel leakage and burn-through are repaired by welding using steel plates of the same material as the furnace shell.

[0081] 4-4) Maintenance of steel leakage and burn-through parts in the converter cap area:

[0082] 4-4-1) If the steel is leaking and burning through in the furnace cap area on the slag pouring side, shake the converter to the front platform to -90°~-100°; if the steel is leaking and burning through in the furnace cap area on the steel tapping side, shake the converter to the rear platform to 90°~100°, use a furnace repair shovel to deliver magnesia carbon bricks from the furnace mouth to the damaged lining position in the furnace for brick laying maintenance, and repeat the above-mentioned brick laying maintenance operation until the damaged lining in the converter cap area is filled and leveled.

[0083] 4-4-2) After the tile maintenance work is completed, the wet gunning process is used, and the compressed air pressure of the PB-II gunning tank is controlled at 0.3~0.5MPa. The magnesium calcium gunning material and water are mixed at a weight ratio of 1:1.0~1:1.3 through a special gunning gun, and the magnesium calcium gunning material is evenly and completely covered with the magnesium carbon bricks. The purpose is to fill the gaps between the magnesium carbon bricks after the patching, and improve the density and thermal shock resistance of the magnesium carbon after sintering. After the gunning operation is completed, the sintering temperature is ≥1620℃, and the sintering time is controlled at 20~25min.

[0084] 4-4-3) After the magnesium-calcium gunning material is fully sintered, if the furnace cap area on the slag pouring side is leaking and burning through, the converter is shaken to 90°~100° towards the rear platform of the furnace; if the furnace cap area on the steel tapping side is leaking and burning through, the converter is shaken to -90°~-100° towards the front platform of the furnace, and the compressed air pressure of the Xuda PZ-3 refractory material spraying machine is controlled at 0.2~0.4MPa. The chrome corundum castable and water are mixed at a weight ratio of 1:0.30~1:0.35 through a special spraying gun, and the chrome corundum slurry is sprayed from the outside of the furnace shell into the leaking and burning part of the furnace body in the furnace cap area of ​​the converter to fill and compact the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 280~400℃, and the sintering time is controlled at 30~40min.

[0085] 4-4-4) After the chrome corundum slurry is fully sintered, if the furnace cap area on the slag pouring side is leaking and burning through, the converter will be shaken to the rear platform at 140°~150°; if the furnace cap area on the steel tapping side is leaking and burning through, the converter will be shaken to the front platform at -140°~-150°, a maintenance work platform will be built, and the furnace shell of the converter cap area where the steel is leaking and burning through will be welded with steel plates of the same material as the furnace shell.

[0086] 4-5) Maintenance of steel leakage and burn-through parts in the bottom area of ​​the converter

[0087] 4-5-1) Shake the converter to -50°~-60° on the platform in front of the furnace, and use a scrap steel bucket to add the converter sand from the converter mouth into the furnace. The reference amount of converter sand is 1000~1200kg. Then, with the zero position (vertical state) as the reference, shake the converter to an angle of -30° in front of the furnace and 30° in back of the furnace. Shake the furnace repeatedly 2~3 times to ensure that the converter sand is completely spread and covers the damaged lining of the converter bottom where steel leaks and burns through. The sintering temperature is ≥1620℃ and the sintering time is controlled at 50~60min.

[0088] 4-5-2) After the converter sand is fully sintered, the converter is shaken to 90°~100° on the rear platform or -90°~-100° on the front platform. The compressed air pressure of the Xuda PZ-3 refractory concrete spraying machine is controlled at 0.2~0.4MPa. The chrome corundum castable and water are mixed at a weight ratio of 1:0.30~1:0.35 through a concrete spraying gun. Then, the chrome corundum slurry is sprayed from the outside of the furnace shell into the steel leakage and burnt-through parts of the converter bottom area to fill and compact the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 280~400℃ and the sintering time is controlled at 30~40min.

[0089] 4-5-3) After the chrome corundum slurry is fully sintered, the converter is tilted to 90°~100° towards the rear platform or -90°~-100° towards the front platform, and a maintenance work platform is built. The furnace shell of the converter bottom area with leaking steel and burned through parts is welded and repaired with steel plates of the same material as the furnace shell.

[0090] 5) Converter resumes production:

[0091] After the furnace shell welding repair of the steel leakage and burnt-through parts of the converter body was completed, the converter resumed normal production.

[0092] 6) Confirm the maintenance effect:

[0093] After the converter has smelted one batch of steel normally and the converter has performed normal slag splashing and furnace protection operations, the slag in the furnace is emptied and the thickness of the lining bricks at the steel leakage site of the converter body is measured again using a Lacam M3 laser thickness gauge to evaluate the maintenance effect and provide a reference for subsequent maintenance of the lining at the steel leakage and burn-through site of the converter body.

[0094] Several specific embodiments of the present invention are as follows:

[0095] Example 1

[0096] A method for maintaining a steel leaking burn-through part of a converter body is to maintain a steel leaking burn-through part of a converter body on a slag pouring side, comprising the following steps:

[0097] 1) When the accident of steel leakage and burning through the furnace body on the slag pouring side of the converter occurs, the converter tilts to the steel tapping side, and cooperates with the ladle car under the furnace to turn the molten steel and slag in the furnace into the ladle from the furnace mouth. The converter is shaken at an angle of 180° to empty the molten steel and slag in the furnace.

[0098] 2) After the molten steel and slag in the converter were emptied, the Lacam M3 laser thickness gauge was used to measure the residual thickness of the furnace lining bricks at the steel leakage part of the converter body on the slag pouring side and the position of steel leakage burn-through. The measured residual thickness of the steel leakage part of the converter body was 20mm, located in the middle of the molten pool on the slag pouring side of the converter. The amount of magnesia carbon bricks used for maintenance was determined to be 260kg.

[0099] 3) The steel leakage and burn-through parts of the furnace body on the slag pouring side of the converter are maintained in accordance with the order of "internal repair first and external repair later" and the principle of "high-temperature hot repair". The internal part adopts the method of "patching magnesia-carbon bricks + magnesia-calcium gunning material wet gunning repair", and the external part adopts the method of "spraying chrome corundum slurry + furnace shell welding repair". The two methods are combined to maintain the steel leakage and burn-through parts of the furnace body on the slag pouring side of the converter, which specifically includes the following steps:

[0100] 3-1) The converter is tilted to -90° toward the platform in front of the furnace, and the magnesia carbon bricks are delivered from the furnace mouth to the damaged lining in the middle of the molten pool on the slag pouring surface of the furnace for brick laying maintenance. Repeat the above-mentioned brick laying maintenance operation until the damaged lining at the location of the leaking steel is filled.

[0101] 3-2) After the tile maintenance work is completed, the wet gunning process is adopted, and the compressed air pressure of the PB-II gunning tank is controlled at 0.3MPa. The magnesium-calcium gunning material and water are mixed in a weight ratio of 1:1.2 through a gunning gun. The magnesium-calcium gunning material is evenly and completely covered with the magnesium-carbon bricks, and the gaps between the magnesium-carbon bricks after the patching are filled. The sintering temperature is 1630℃ and the sintering time is 20min.

[0102] 3-3) After the magnesium-calcium gunning material is fully sintered, the converter is shaken to 150° toward the rear platform of the furnace, and the compressed air pressure of the Xuda brand PZ-3 refractory concrete spraying machine is controlled at 0.3MPa. The chrome corundum castable and water are mixed in a weight ratio of 1:0.30 through a concrete spraying gun. Then, the chrome corundum slurry is sprayed from the outside of the furnace shell into the steel leakage and burnt-through part of the furnace body in the middle of the molten pool on the slag pouring side of the converter to fill and compact the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 300℃ and the sintering time is controlled at 30min.

[0103] 3-4) After the chrome corundum slurry is fully sintered, the converter is shaken to 150 degrees toward the platform behind the furnace, and a maintenance work platform is built. The furnace shell of the converter with the same material as the furnace shell is welded and repaired at the leaking and burning part of the furnace body in the middle of the molten pool on the slag pouring side of the converter.

[0104] 4) After the furnace shell welding repair of the furnace body leakage and burn-through part in the middle of the molten pool on the slag pouring side of the converter was completed, the converter resumed normal production.

[0105] 5) After the converter smelted one batch of steel normally, no furnace shell burning and steel leakage were found in this place during the smelting process. After the converter was operated normally with slag splashing, the slag in the furnace was turned over and the Lacam M3 laser thickness gauge was used to measure again. The actual thickness of the furnace lining brick at the steel leakage and burning point in the middle of the molten pool on the slag pouring side of the converter was 600mm. The maintenance effect was good and the maintenance work was completed.

[0106] Example 2

[0107] A method for maintaining a steel leaking burn-through portion of a converter body, for maintaining a steel leaking burn-through portion of a converter body on a steel tapping side, specifically comprising the following steps:

[0108] 1) When the converter body leaks and burns through on the steel-out side, the converter tilts to the slag-discharging side, and cooperates with the ladle car under the furnace to turn the molten steel and slag in the furnace into the ladle from the furnace mouth. The converter is shaken at a reference angle of -180° to empty the molten steel and slag in the furnace.

[0109] 2) After the molten steel and slag in the converter furnace were emptied, the Lacam M3 laser thickness gauge was used to measure the residual thickness of the lining bricks at the steel leakage part of the converter body and the position of the steel leakage burn-through. The measured residual thickness of the lining bricks at the steel leakage part of the converter body was 50mm, located at the lower right corner of the steel tapping side of the converter. The amount of magnesia carbon bricks used for maintenance was determined to be 240kg.

[0110] 3) Maintain the steel leakage and burn-through parts of the converter body on the steel-outlet side in accordance with the order of "internal repair first and external repair later" and the principle of "high-temperature hot repair". The internal part adopts the method of "patching magnesia-carbon bricks + magnesia-calcium gunning material wet gunning repair", and the external part adopts the method of "spraying chrome corundum slurry + furnace shell welding repair". The two methods are combined to maintain the steel leakage and burn-through parts of the converter body. The specific process is:

[0111] 3-1) The converter is tilted to 100° toward the rear platform of the furnace, and the magnesia carbon bricks are delivered from the furnace mouth to the damaged lining position at the lower right corner of the steel-outlet side of the furnace using a furnace repair shovel for brick laying maintenance. Repeat the aforementioned brick laying maintenance operation until the damaged lining at the lower right corner of the converter steel-outlet side where the furnace body is leaking and burning through is filled.

[0112] 3-2) After the tile maintenance work is completed, the wet gunning process is adopted, and the compressed air pressure of the PB-II gunning tank is controlled at 0.4MPa. The magnesium-calcium gunning material and water are mixed in a weight ratio of 1:1.2 through a gunning gun. The magnesium-calcium gunning material is evenly and completely covered with the magnesium-carbon bricks, and the gaps between the magnesium-carbon bricks after the patching are filled. The sintering temperature is 1620℃ and the sintering time is 20min.

[0113] 3-3) After the magnesium-calcium gunning material is fully sintered, the converter is shaken to -150° towards the platform in front of the furnace, and the compressed air pressure of the Xuda PZ-3 refractory concrete spraying machine is controlled at 0.3MPa. The chrome corundum castable and water are mixed in a weight ratio of 1:0.32 through a concrete spraying gun. Then, the chrome corundum slurry is sprayed from the outside of the furnace shell into the steel leakage and burnt-through part of the furnace body at the lower right corner of the steel-out side of the converter to fill and compact the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 320℃ and the sintering time is controlled at 30min.

[0114] 3-4) After the chrome corundum slurry is fully sintered, the converter is shaken to -150° towards the platform in front of the furnace, and a maintenance work platform is built. The furnace shell of the converter at the lower right corner of the steel-out side where the furnace body is leaking and burned through is welded using a steel plate of the same material as the furnace shell.

[0115] 4) After the furnace shell welding repair at the part where steel was leaking and burned through at the lower right corner of the converter's steel-out side was completed, the converter resumed normal production.

[0116] 5) After the converter smelted one batch of steel normally, no furnace shell burning and steel leakage were found in this place during the smelting process. After the converter was operated normally with slag splashing, the slag in the furnace was turned over and the Lacam M3 laser thickness gauge was used to measure again. The actual thickness of the furnace lining brick at the bottom right corner of the steel-outlet side of the converter after maintenance was 620mm, and the maintenance effect was good. The maintenance work was completed.

[0117] Example 3

[0118] A method for maintaining the steel leakage and burn-through part of the converter body, which is aimed at maintaining the steel leakage and burn-through part of the converter body in the right ear shaft area. The specific method is:

[0119] 1) When the furnace body leaks and burns through the right ear shaft area of ​​the converter, the converter tilts to the slag discharge side, and cooperates with the ladle car under the furnace to turn the molten steel and slag in the furnace into the ladle from the furnace mouth. The reference angle of the converter shaking is -180° to empty the molten steel and slag in the furnace.

[0120] 2) After the molten steel and slag in the converter were emptied, the Lacam M3 laser thickness gauge was used to measure the residual thickness and position of the lining bricks at the leaky and burnt-through parts of the converter body in the trunnion area. The measured residual thickness of the lining bricks at the leaky part of the converter body was 40mm, located at the slag line of the trunnion on the right side of the converter. The amount of magnesia carbon bricks used for maintenance was determined to be 260kg.

[0121] 3) The steel leakage and burn-through parts of the converter body are maintained in accordance with the order of "internal repair first and external repair later" and the principle of "high-temperature hot repair". The internal part adopts the method of "patching magnesia carbon bricks + magnesia calcium gunning material wet gunning repair", and the external part adopts the method of "spraying chrome corundum mud + furnace shell welding repair". The two methods are combined to maintain the steel leakage and burn-through parts of the converter body. The specific process is:

[0122] 3-1) The converter is tilted to -90° toward the platform in front of the furnace, and the magnesia carbon bricks are delivered from the furnace mouth to the damaged lining position in the furnace using a furnace repair shovel for brick laying maintenance. The aforementioned brick laying maintenance operation is repeated until the damaged lining at the position where the slag line of the right ear shaft of the converter is leaked and burned through is filled.

[0123] 3-2) After the maintenance work of tiling is completed, the wet gunning process is adopted, and the compressed air pressure of the PB-II gunning tank is controlled at 0.4MPa. The magnesium calcium gunning material and water are mixed at a weight ratio of 1:1.2 through the gunning gun, and the magnesium calcium gunning material is evenly and completely covered with the magnesium carbon bricks. The purpose is to fill the gaps between the magnesium carbon bricks after the patching, and improve the density and thermal shock resistance of magnesium carbon after sintering. After the gunning operation is completed, the temperature is 1640℃ and the sintering time is controlled at 25min.

[0124] 3-3) After the magnesium-calcium gunning material is fully sintered, the converter is shaken to 90 degrees toward the platform behind the furnace, and the compressed air pressure of the Xuda brand PZ-3 refractory material spraying machine is controlled at 0.4MPa. The chrome corundum castable and water are mixed in a weight ratio of 1:0.33 through a spray gun. Then, the chrome corundum slurry is sprayed from the outside of the furnace shell into the steel leakage and burnt-through part of the slag line of the ear shaft on the right side of the converter to fill and compact the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 380℃ and the sintering time is controlled at 30min.

[0125] 3-4) After the chrome corundum slurry is fully sintered, the converter is shaken to 90 degrees toward the platform behind the furnace, and a maintenance work platform is built. The furnace shell of the right ear shaft area of ​​the converter where steel is leaking and burned through is welded using steel plates of the same material as the furnace shell.

[0126] 4) After the furnace shell welding repair of the steel leakage and burn-through area in the right ear shaft area of ​​the converter was completed, the converter resumed normal production.

[0127] 5) After the converter smelted one batch of steel normally, no furnace shell burning and steel leakage were found in this area during the smelting process. After the converter was operated normally with slag splashing, the slag in the furnace was turned over and the Lacam M3 laser thickness gauge was used to measure again. The actual measurement showed that the thickness of the furnace lining bricks in the steel leakage and burn-through area of ​​the right ear shaft area of ​​the converter after maintenance was 640mm. The maintenance effect was good and the maintenance work was completed.

[0128] Example 4

[0129] A method for maintaining a steel leaking burn-through part of a converter body, which is aimed at maintaining a steel leaking burn-through part of a converter body in a furnace cap area on a slag pouring side, specifically comprises the following steps:

[0130] 1) When the accident of steel leakage and burning through of the furnace body in the furnace cap area on the slag pouring side of the converter occurs, the converter tilts to the steel tapping side, and cooperates with the ladle car under the furnace to turn the molten steel and slag in the furnace into the ladle from the furnace mouth. The converter is shaken at a reference angle of 180° to empty the molten steel and slag in the furnace.

[0131] 2) After the molten steel and slag in the converter were emptied, the Lacam M3 laser thickness gauge was used to measure the residual thickness and position of the lining bricks at the leaking and burning-through parts of the converter body in the cap area. The measured residual thickness of the lining bricks at the leaking part of the converter body was 20mm, located in the middle of the cap on the slag pouring side of the converter. The amount of magnesia carbon bricks used for maintenance was determined to be 260kg.

[0132] 3) According to the order of "internal repair first and external repair later" and the principle of "high temperature hot repair", the steel leakage and burn-through part of the furnace body in the middle of the furnace cap on the slag pouring side of the converter is maintained. The internal part adopts the method of "patching magnesia carbon bricks + magnesia calcium gunning material wet gunning repair", and the external part adopts the method of "spraying chrome corundum mud + furnace shell welding repair". The two methods are combined to maintain the steel leakage and burn-through part of the converter body. The specific process is as follows:

[0133] 3-1) The converter is tilted to -90° toward the platform in front of the furnace, and the magnesia carbon bricks are delivered from the furnace mouth to the damaged lining position in the furnace using a furnace repair shovel for brick laying maintenance. The aforementioned brick laying maintenance operation is repeated until the damaged lining at the center of the furnace cap on the slag pouring side of the converter is filled.

[0134] 3-2) After the tile maintenance work is completed, the wet gunning process is used, the compressed air pressure of the PB-II gunning tank is controlled at 0.4MPa, the magnesium calcium gunning material and water are mixed at a weight ratio of 1:1.3 through the gunning gun, and the magnesium calcium gunning material is evenly and completely covered with the magnesium carbon bricks. The purpose is to fill the gaps between the magnesium carbon bricks after the patching, and improve the density and thermal shock resistance of the magnesium carbon after sintering. After the gunning operation is completed, the temperature is 1640℃ and the sintering time is controlled at 20min.

[0135] 3-3) After the magnesium-calcium gunning material is fully sintered, the converter is shaken to 100° toward the rear platform of the furnace, and the compressed air pressure of the Xuda brand PZ-3 refractory material spraying machine is controlled at 0.4MPa. The chrome corundum castable and water are mixed in a weight ratio of 1:0.32 through a spray gun. Then, the chrome corundum slurry is sprayed from the outside of the furnace shell into the steel leakage and burnt-through area in the middle of the furnace cap area on the slag pouring side of the converter to fill and compact the gap between the furnace shell steel plate and the furnace lining. The temperature is 400℃ and the sintering time is controlled at 30min.

[0136] 3-4) After the chrome corundum slurry is fully sintered, the converter is shaken to 150 degrees toward the platform behind the furnace, and a maintenance work platform is built. The furnace shell is welded with a steel plate of the same material as the furnace shell to repair the steel leakage and burn-through part in the middle of the furnace cap area on the slag pouring side of the converter.

[0137] 4) After the furnace shell welding repair of the steel leakage and burn-through part in the center of the furnace cap area on the slag pouring side of the converter was completed, the converter resumed normal production.

[0138] 5) After the converter smelted one batch of steel normally, no furnace shell burning and steel leakage were found in this area during the smelting process. After the converter was operated normally with slag splashing, the slag in the furnace was turned over and the Lacam M3 laser thickness gauge was used to measure again. The actual measurement showed that the thickness of the furnace lining brick at the steel leakage and burn-through position in the middle of the furnace cap area on the slag pouring side of the converter after maintenance was 650mm. The maintenance effect was good and the maintenance work was completed.

[0139] Example 5

[0140] A method for maintaining a steel leaking burn-through part of a converter body, targeting at maintaining a steel leaking burn-through part of a converter bottom area, comprises the following steps:

[0141] 1) When the converter bottom leaks and burns through accident occurs, the converter tilts to the slag discharge side, and cooperates with the ladle car under the furnace to turn the molten steel and slag in the furnace into the ladle from the furnace mouth. The converter is shaken at a reference angle of -180° to empty the molten steel and slag in the furnace.

[0142] 2) Maintain the steel leakage and burn-through parts of the converter furnace body in the bottom area of ​​the converter in the order of "internal repair first and external repair later" and the principle of "high temperature hot repair". The internal part adopts the "converter sand hot repair" method, and the external part adopts the "chrome corundum slurry injection + furnace shell welding repair" method. The two methods are combined to maintain the steel leakage and burn-through parts of the converter furnace body at the bottom of the converter. The specific process is as follows:

[0143] 2-1) Shake the converter to -60° toward the platform in front of the furnace, use a scrap steel bucket to add the converter sand into the converter, the amount of converter sand is 1200kg, and then the converter is shaken to -30° toward the front of the furnace and 30° toward the back of the furnace based on the zero position (vertical state), and shake the furnace repeatedly for 2 times to ensure that the converter sand is completely spread and covers the damaged lining of the converter bottom where the steel leaks and burns through. The sintering temperature is 1638℃ and the sintering time is controlled at 60min.

[0144] 2-2) After the converter sand is fully sintered, the converter is shaken to 90 degrees to the back of the furnace, and the compressed air pressure of the Xuda PZ-3 refractory material spraying machine is controlled at 0.3MPa. The chrome corundum castable and water are mixed in a weight ratio of 1:0.33 through a spray gun. Then, the chrome corundum slurry is sprayed from the outside of the furnace shell into the steel leakage and burnt-through parts of the converter bottom area to fill and compact the gap between the furnace shell steel plate and the furnace lining. The sintering temperature is 400℃ and the sintering time is controlled at 40min.

[0145] 2-3) After the chrome corundum slurry is fully sintered, the converter is swung to 90 degrees to the rear of the furnace, and a maintenance work platform is built. The furnace shell of the converter bottom area where steel is leaking and burned through is welded using steel plates of the same material as the furnace shell.

[0146] 3) After the furnace shell welding repair of the steel leakage and burnt-through parts in the converter bottom area was completed, the converter resumed normal production.

[0147] 4) After the converter smelted one batch of steel normally, no furnace shell burning and steel leakage were found in this area during the smelting process. After the converter was operated normally with slag splashing, the slag in the furnace was turned over and the Lacam M3 laser thickness gauge was used to measure again. The actual measurement showed that the thickness of the furnace lining brick at the location of the converter bottom steel leakage and burn-through after maintenance was 610mm, and the maintenance effect was good, and the maintenance work was completed.

[0148] The present invention aims to solve the technical problems that the maintenance process of the steel leakage and burn-through parts of the converter body is difficult, time-consuming and the maintenance effect is poor, and adopts a highly targeted maintenance operation method: (1) According to the different steel leakage and burn-through parts of the furnace body, the corresponding molten steel and slag emptying and furnace shutdown operation is adopted to avoid the aggravation of the damage of the steel leakage and burn-through parts of the furnace body; (2) The LacamM3 laser thickness gauge is used to measure the residual thickness of the furnace lining bricks and the steel leakage position of the furnace body leakage and burn-through parts to determine the amount of magnesium carbon bricks used for maintenance and the specific maintenance position, so as to provide a reference for the maintenance of the steel leakage and burn-through parts of the converter body; (3) The magnesium carbon bricks used for maintenance inside the converter are consistent with the material of the original converter lining bricks, which effectively avoids the influence of thermal expansion degree differences on the maintenance effect; chrome corundum castable with high compressive strength and refractoriness is selected for the outside, and a concrete spraying machine is used to spray chrome corundum slurry into the steel leakage and burn-through parts of the furnace body The parts are conducive to filling and compacting the gap between the furnace shell and the furnace lining bricks. The outermost part is welded with steel plates of the same material as the original furnace shell to provide support and protection and prevent the chrome corundum castable from powdering and falling off after injection and sintering; (4) According to the difficulty of maintaining the steel leakage and burn-through parts of the converter body, the steel leakage and burn-through parts of the converter body are maintained in the order of "internal repair first and external repair later" and the principle of "high-temperature hot repair". The internal parts are repaired by "magnesium carbon bricks + magnesium calcium spraying material wet spraying" and "converter sand hot repair". The external parts are repaired by "spraying chrome corundum mud + furnace shell welding". The two are combined to maintain the steel leakage and burn-through parts of the converter body. During the process, the sintering temperature and sintering time of the refractory after different maintenance are reasonably limited, which effectively improves the maintenance quality of the steel leakage and burn-through parts of the converter body; (5) After the converter has smelted one batch of steel normally, Lacam is used The M3 laser thickness gauge was used to measure the thickness of the lining bricks at the leaking parts of the converter body again to evaluate the maintenance effect and provide a reference for the subsequent maintenance of the lining at the leaking and burn-through parts of the converter body.

[0149] Comparative Example 1

[0150] A method for maintaining a steel leaking burn-through part of a converter body, which is aimed at maintaining a steel leaking burn-through part of a converter body in a furnace cap area on a slag pouring side, specifically comprises the following steps:

[0151] 1) When the accident of steel leakage and burning through of the furnace body in the furnace cap area on the slag pouring side of the converter occurs, the converter tilts to the steel tapping side, and cooperates with the ladle car under the furnace to turn the molten steel and slag in the furnace into the ladle from the furnace mouth. The converter is shaken at a reference angle of 180° to empty the molten steel and slag in the furnace.

[0152] 2) After the molten steel and slag in the converter furnace were emptied, the Lacam M3 laser thickness gauge was used to measure the residual thickness and position of the lining bricks at the leaking and burning-through parts of the converter body in the furnace cap area. The measured residual thickness of the lining bricks at the leaking part of the converter body was 50mm, located in the middle of the cap on the slag pouring side of the converter. The amount of magnesia carbon bricks used for maintenance was determined to be 240kg.

[0153] 3) The internal method of "patching magnesia carbon bricks + magnesia calcium gunning material wet gunning" was adopted, and the external method of "spraying chrome corundum mud" was not adopted to maintain the steel leakage and burn-through parts of the converter body. The specific process is as follows:

[0154] 3-1) The converter is tilted to -90° toward the platform in front of the furnace, and the magnesia carbon bricks are delivered from the furnace mouth to the damaged lining position in the furnace using a furnace repair shovel for brick laying maintenance. The aforementioned brick laying maintenance operation is repeated until the damaged lining at the center of the furnace cap on the slag pouring side of the converter is filled.

[0155] 3-2) After the tile maintenance work is completed, the wet gunning process is used, and the compressed air pressure of the PB-II gunning tank is controlled at 0.4MPa. The magnesium-calcium gunning material and water are mixed at a weight ratio of 1:1.3 through the gunning gun, and the magnesium-calcium gunning material is evenly and completely covered with the magnesium-carbon bricks. The purpose is to fill the gaps between the magnesium-carbon bricks after the patching, and improve the density and thermal shock resistance of the magnesium-carbon sintering. After the gunning operation is completed, the sintering temperature is 1620℃, and the sintering time is controlled at 20min.

[0156] 3-3) After the magnesium-calcium gunning material is fully sintered, the converter is shaken to 150 degrees toward the platform behind the furnace, and a maintenance work platform is built. The furnace shell is welded with a steel plate of the same material as the furnace shell to repair the steel leakage and burn-through part in the middle of the furnace cap area on the slag pouring side of the converter.

[0157] 4) After the furnace shell welding repair of the steel leakage and burn-through parts in the furnace cap area on the slag pouring side of the converter was completed, the converter resumed normal production.

[0158] 5) Because the outside of the converter body did not adopt the "chrome corundum slurry injection + furnace shell welding repair" method, the gap between the furnace shell and the furnace lining could not be filled, and there was no supporting protection. During the normal smelting of one batch of steel in the converter, the furnace shell burned red and steel leaked again.

[0159] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for maintaining the burn-through position of a converter body, characterized in that: The converter body leak-through location maintenance method comprises the following steps: 1) When the converter body leaks and burns through, empty the molten steel and slag in the converter and shut down the furnace; 2) Measure the residual thickness and damaged position of the furnace lining bricks at the leaky and burnt-through parts of the converter body, and determine the amount of maintenance materials and the specific maintenance location; 3) First, maintain and sinter the damaged lining of the converter body where steel leaks and burns through; 4) Mix the chrome corundum castable with water to make chrome corundum slurry, and spray the chrome corundum slurry into the steel leakage and burn-through parts of the converter body from the external furnace shell to fill and compact the gap between the furnace shell steel plate and the furnace lining for sintering; 5) Finally, the furnace shell of the converter body where steel has leaked and burned through is repaired by welding.

2. The method for maintaining the burn-through position of the converter body according to claim 1 is characterized in that: In step 1), when a steel leakage and burn-through accident occurs on the slag pouring side of the converter, the converter is tilted toward the steel tapping side, and the molten steel and slag in the furnace are turned into the ladle from the furnace mouth and emptied; Or, when the furnace body leaks and burns through the converter on the steel tapping side, the converter tilts toward the slag dumping side, pouring the molten steel and slag in the furnace from the furnace mouth into the ladle and emptying it; Or, when the furnace body leaks and burns through the converter trunnion area, the converter tilts toward the slag pouring side or the steel tapping side, and the molten steel and slag in the furnace are turned into the ladle from the furnace mouth and emptied; Or, when a steel leakage and burn-through accident occurs in the furnace cap area on the slag pouring side of the converter, the converter tilts toward the steel tapping side, and the molten steel and slag in the furnace are turned into the ladle from the furnace mouth and then turned empty; Or, when a steel leakage and burn-through accident occurs in the furnace cap area on the steel tapping side of the converter, the converter tilts toward the slag dumping side, and the molten steel and slag in the furnace are dumped into the ladle from the furnace mouth and then emptied; Or, when a steel leakage and burn-through accident occurs in the bottom area of ​​the converter, the converter tilts to the slag pouring side or the steel tapping side, and the molten steel and slag in the furnace are poured into the ladle from the furnace mouth and emptied.

3. The method for maintaining the burn-through position of the converter body according to claim 1, characterized in that: In step 2), the maintenance materials include magnesia carbon bricks, converter sand, magnesia calcium gunning material and chrome corundum castable.

4. The method for maintaining the burn-through position of the converter body according to claim 1, characterized in that: In step 3), the damaged lining of the converter body where steel leaks and burns through is first maintained from the inside, specifically: When steel leakage and burning through occur in the furnace body on the slag pouring side of the converter, the furnace body on the steel tapping side, the furnace body in the converter ear shaft area, the furnace cap area on the slag pouring side of the converter and the furnace cap area on the steel tapping side of the converter, first use magnesia carbon bricks to maintain the damaged lining position in the furnace, and then use magnesia calcium gunning material mixed with water for gunning to fill the gaps between the magnesia carbon bricks after gunning, and then sintering is carried out. The sintering temperature is ≥1620℃ and the sintering time is 20-25min.

5. The method for maintaining the burn-through position of the converter body according to claim 4, characterized in that: In step 3), the weight ratio of the magnesium-calcium gunning material to water is 1:1.0 to 1:1.3, and the gunning pressure is controlled at 0.3 to 0.5 MPa.

6. The method for maintaining the burn-through position of the converter body according to claim 1, characterized in that: When steel leakage and burn-through occur in the bottom area of ​​the converter, add converter sand into the furnace from the converter mouth, and then shake the converter to an angle of -30°~30° towards the front and back of the furnace based on the zero position. Shake the furnace repeatedly 2~3 times to ensure that the converter sand is completely spread and covers the damaged lining at the leaking and burn-through area of ​​the converter bottom, and then sintering is carried out. The sintering temperature is ≥1620℃ and the sintering time is 50~60min.

7. The method for maintaining the burn-through position of the converter body according to claim 1, characterized in that: In step 4), the mass ratio of the chrome corundum castable to water is 1:0.30 to 1:0.

35.

8. The method for maintaining the burn-through position of the converter body according to claim 1 or 7, characterized in that: In step 4), the pressure of the chrome corundum slurry injection is controlled at 0.2-0.4 MPa.

9. The method for maintaining the burn-through position of the converter body according to claim 1 or 7, characterized in that: In step 4), the sintering temperature is 280-400° C. and the sintering time is 30-40 minutes.

10. The method for maintaining the steel leakage burn-through part of the converter body according to claim 1, in step 5), the converter shell at the steel leakage burn-through part is welded with a steel plate of the same material as the furnace shell.

Citation Information

Patent Citations

  • Device and method for monitoring the erosion state of a converter lining on line in real time

    CN110453034A

  • On-line repair method for perforation of converter body

    CN110653450A

  • Method for early warning risk of bleed-out near bottom blowing brick of converter

    CN111850230A

  • Repairing method for molten metal vessel

    JP1994313682A

  • Castable refractory used for mending of immersion tube for degassing by spray

    JP2017150042A