Method for improving purity of molten steel based on slag component control
By adjusting the slag composition and using deoxidants, combined with refining technology, the problem of controlling the purity of molten steel is solved, the quality and performance of steel is significantly improved, and the needs of high-end special steels are met.
Patent Information
- Application Number
- CN202411167903.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The purity of molten steel is difficult to effectively control during steelmaking, resulting in limited mechanical properties and fatigue life of steel, affecting the development of high-end special steels.
By adjusting the ratio of CaO, SiO2, Al2O3, MgO in the slag, controlling the weight ratio of CaO and SiO2, and adding a deoxidant before the steel is discharged, refining technology is used to reduce the gas content and inclusions in the molten steel, and promoting its reaction with the slag and Remove.
Effectively remove impurities, such as sulfur and phosphorus, reduce the formation of oxide inclusions, protect the molten steel from secondary oxidation, and improve the quality and performance of the final product.
Smart Images

Figure BDA0005008361940000111 
Figure BDA0005008361940000121
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steelmaking, and in particular to a method for improving the purity of molten steel based on slag composition control. Background Art
[0002] Special steel is a steel material with special uses. It is generally used to process key components with special performance requirements in high-end manufacturing equipment, such as wheels, rails, shafts, springs, gears, bearings and connectors. It is the most important steel material for the development of modern manufacturing. The purity of molten steel is an important indicator of the quality level of special steel. It directly affects the mechanical properties and fatigue life of steel, and is also the main factor restricting the development of high-end special steel in my country. The total oxygen and inclusions in steel are the main indicators to measure the purity control. As the oxygen content decreases and the size of non-metallic inclusions decreases, the fatigue life of steel parts increases exponentially.
[0003] Improving the purity of molten steel based on slag composition control is a very important part of the steelmaking process. Reasonable slag composition can not only help remove impurities in molten steel, but also protect the molten steel from secondary oxidation, thereby improving the quality of the final product. Summary of the invention
[0004] In order to solve at least one of the above technical problems, a method for improving the purity of molten steel is developed. The present application provides a method for improving the purity of molten steel based on slag composition control.
[0005] The present application provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0006] S1. Optimize slag composition
[0007] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0008] S2. Control the basicity of slag
[0009] Adjustment of CaO and SiO 2 Weight ratio;
[0010] S3, add deoxidizer:
[0011] Add deoxidizer before tapping;
[0012] S4, Refining
[0013] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0014] By adopting the above technical solution, the CaO and SiO in the slag are adjusted. 2 、Al 2 O 3 , MgO ratio, adjust CaO and SiO 2 By adding deoxidizer before steelmaking, and using refining technology to reduce the gas content in the molten steel, it can not only remove the impurity elements (such as sulfur, phosphorus, etc.) in the molten steel, but also protect the molten steel from secondary oxidation, thereby improving the quality of the final product.
[0015] Optionally, in S1, the CaO, SiO 2 、Al2O 3 , MgO are respectively in parts by weight: CaO 40-60 parts, SiO 2 13-20 parts, Al 2 O 3 5 to 15 parts, MgO 5 to 20 parts.
[0016] By adopting the above technical solutions, the best fluidity, alkalinity and reducibility can be obtained, thereby improving the desulfurization and dephosphorization efficiency.
[0017] Optionally, in the S2, the CaO and SiO 2 The weight ratio is 2.0 to 4.6.
[0018] By adopting the above technical solution, the CaO and SiO 2 The basicity of the slag can be controlled by
[0019] Optionally, in the S2, the CaO and SiO 2 The weight ratio is 3.
[0020] By adopting the above technical solution, the optimal slag basicity is selected to further promote desulfurization, dephosphorization and other reactions.
[0021] Optionally, the deoxidizer is aluminum or ferrosilicon.
[0022] By adopting the above technical solution, the dissolved oxygen content in molten steel can be effectively reduced, thereby reducing the formation of oxide inclusions.
[0023] Optionally, the refining technology adopts: vacuum degassing (VD), vacuum argon blowing (RH).
[0024] By adopting the above technical solution, the floating of inclusions is promoted.
[0025] Optionally, the stirring method adopts: ladle argon blowing (SLF) or top argon blowing (TBF).
[0026] By adopting the above technical solution, the reaction between inclusions and slag and the removal of inclusions are accelerated.
[0027] In summary, the present invention adjusts the CaO and SiO in the slag. 2 、Al 2 O 3 , MgO ratio, adjust CaO and SiO 2 By adding deoxidizer before steelmaking, and using refining technology to reduce the gas content in the molten steel, it can not only remove the impurity elements (such as sulfur, phosphorus, etc.) in the molten steel, but also protect the molten steel from secondary oxidation, thereby improving the quality of the final product. DETAILED DESCRIPTION
[0028] The present application is further described in detail below with reference to the embodiments.
[0029] In the following examples of the present application, the main components involved, unless otherwise specified, were purchased from commercially available products.
[0030] Example 1
[0031] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0032] S1. Optimize slag composition
[0033] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0034] S2. Control the basicity of slag
[0035] Adjustment of CaO and SiO 2 Weight ratio;
[0036] S3, add deoxidizer:
[0037] Add deoxidizer before tapping;
[0038] S4, Refining
[0039] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0040] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 40 parts, SiO 2 20 parts, Al 2 O 35 parts, MgO 10 parts.
[0041] In this embodiment, CaO and SiO 2 The weight ratio is 2.0.
[0042] In this embodiment, aluminum is used as the deoxidizer.
[0043] In this embodiment, the refining technology used is: vacuum degassing (VD).
[0044] In this embodiment, the stirring method adopted is: ladle argon blowing (SLF).
[0045] Example 2
[0046] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0047] S1. Optimize slag composition
[0048] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0049] S2. Control the basicity of slag
[0050] Adjustment of CaO and SiO 2 Weight ratio;
[0051] S3, add deoxidizer:
[0052] Add deoxidizer before tapping;
[0053] S4, Refining
[0054] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0055] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 45 parts, SiO 2 18 copies, Al 2 O 3 10 parts, MgO 15 parts.
[0056] In this embodiment, CaO and SiO 2 The weight ratio is 2.5.
[0057] In this embodiment, aluminum is used as the deoxidizer.
[0058] In this embodiment, the refining technology used is: vacuum degassing (VD).
[0059] In this embodiment, the stirring method adopted is: ladle argon blowing (SLF).
[0060] Example 3
[0061] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0062] S1. Optimize slag composition
[0063] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0064] S2. Control the basicity of slag
[0065] Adjustment of CaO and SiO 2 Weight ratio;
[0066] S3, add deoxidizer:
[0067] Add deoxidizer before tapping;
[0068] S4, Refining
[0069] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0070] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 50 parts, SiO 2 17 copies, Al 2 O 3 15 parts, MgO 20 parts.
[0071] In this embodiment, CaO and SiO 2 The weight ratio is 3.0.
[0072] In this embodiment, aluminum is used as the deoxidizer.
[0073] In this embodiment, the refining technology used is: vacuum degassing (VD).
[0074] In this embodiment, the stirring method adopted is: ladle argon blowing (SLF).
[0075] Example 4
[0076] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0077] S1. Optimize slag composition
[0078] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0079] S2. Control the basicity of slag
[0080] Adjustment of CaO and SiO 2 Weight ratio;
[0081] S3, add deoxidizer:
[0082] Add deoxidizer before tapping;
[0083] S4, Refining
[0084] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0085] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 55 parts, SiO 2 15 copies, Al 2 O 3 10 parts, MgO 5 parts.
[0086] In this embodiment, CaO and SiO 2 The weight ratio is 3.7.
[0087] In this embodiment, aluminum is used as the deoxidizer.
[0088] In this embodiment, the refining technology used is: vacuum degassing (VD).
[0089] In this embodiment, the stirring method adopted is: ladle argon blowing (SLF).
[0090] Example 5
[0091] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0092] S1. Optimize slag composition
[0093] Adjust CaO and SiO in slag 2 、Al 2 O 3, the proportion of MgO;
[0094] S2. Control the basicity of slag
[0095] Adjustment of CaO and SiO 2 Weight ratio;
[0096] S3, add deoxidizer:
[0097] Add deoxidizer before tapping;
[0098] S4, Refining
[0099] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0100] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 60 parts, SiO 2 13 copies, Al 2 O 3 10 parts, MgO 5 parts.
[0101] In this embodiment, CaO and SiO 2 The weight ratio is 4.6.
[0102] In this embodiment, aluminum is used as the deoxidizer.
[0103] In this embodiment, the refining technology used is: vacuum degassing (VD).
[0104] In this embodiment, the stirring method adopted is: ladle argon blowing (SLF).
[0105] Example 6
[0106] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0107] S1. Optimize slag composition
[0108] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0109] S2. Control the basicity of slag
[0110] Adjustment of CaO and SiO 2 Weight ratio;
[0111] S3, add deoxidizer:
[0112] Add deoxidizer before tapping;
[0113] S4, Refining
[0114] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0115] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 40 parts, SiO 2 20 parts, Al 2 O 3 5 parts, MgO 10 parts.
[0116] In this embodiment, CaO and SiO 2 The weight ratio is 2.0.
[0117] In this embodiment, the deoxidizer is ferrosilicon.
[0118] In this embodiment, the refining technology used is: vacuum argon blowing (RH).
[0119] In this embodiment, the stirring method adopted is: top blowing argon (TBF).
[0120] Example 7
[0121] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0122] S1. Optimize slag composition
[0123] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0124] S2. Control the basicity of slag
[0125] Adjustment of CaO and SiO 2 Weight ratio;
[0126] S3, add deoxidizer:
[0127] Add deoxidizer before tapping;
[0128] S4, Refining
[0129] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0130] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 45 parts, SiO 2 18 copies, Al 2 O 3 10 parts, MgO 15 parts.
[0131] In this embodiment, CaO and SiO 2 The weight ratio is 2.5.
[0132] In this embodiment, the deoxidizer is ferrosilicon.
[0133] In this embodiment, the refining technology used is: vacuum argon blowing (RH).
[0134] In this embodiment, the stirring method adopted is: top blowing argon (TBF).
[0135] Example 8
[0136] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0137] S1. Optimize slag composition
[0138] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0139] S2. Control the basicity of slag
[0140] Adjustment of CaO and SiO 2 Weight ratio;
[0141] S3, add deoxidizer:
[0142] Add deoxidizer before tapping;
[0143] S4, Refining
[0144] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0145] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 50 parts, SiO 2 17 copies, Al 2 O 3 15 parts, MgO 20 parts.
[0146] In this embodiment, CaO and SiO 2 The weight ratio is 3.0.
[0147] In this embodiment, the deoxidizer is ferrosilicon.
[0148] In this embodiment, the refining technology used is: vacuum argon blowing (RH).
[0149] In this embodiment, the stirring method adopted is: top blowing argon (TBF).
[0150] Example 9
[0151] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0152] S1. Optimize slag composition
[0153] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0154] S2. Control the basicity of slag
[0155] Adjustment of CaO and SiO 2 Weight ratio;
[0156] S3, add deoxidizer:
[0157] Add deoxidizer before tapping;
[0158] S4, Refining
[0159] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0160] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 55 parts, SiO 2 15 copies, Al 2 O 3 10 parts, MgO 5 parts.
[0161] In this embodiment, CaO and SiO 2 The weight ratio is 3.7.
[0162] In this embodiment, the deoxidizer is ferrosilicon.
[0163] In this embodiment, the refining technology used is: vacuum argon blowing (RH).
[0164] In this embodiment, the stirring method adopted is: top blowing argon (TBF).
[0165] Example 10
[0166] This embodiment provides a method for improving the purity of molten steel based on slag composition control, comprising the following steps:
[0167] S1. Optimize slag composition
[0168] Adjust CaO and SiO in slag 2 、Al 2 O 3 , the proportion of MgO;
[0169] S2. Control the basicity of slag
[0170] Adjustment of CaO and SiO 2 Weight ratio;
[0171] S3, add deoxidizer:
[0172] Add deoxidizer before tapping;
[0173] S4, Refining
[0174] Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
[0175] In this embodiment, CaO, SiO 2 、Al 2 O 3 , MgO by weight: CaO 60 parts, SiO 2 13 copies, Al 2 O 3 10 parts, MgO 5 parts.
[0176] In this embodiment, CaO and SiO 2 The weight ratio is 4.6.
[0177] In this embodiment, the deoxidizer is ferrosilicon.
[0178] In this embodiment, the refining technology used is: vacuum argon blowing (RH).
[0179] In this embodiment, the stirring method adopted is: top blowing argon (TBF).
[0180] The steels prepared in Examples 1 to 10 were tested, and the test results are shown in Table 1.
[0181] Table 1
[0182]
[0183]
[0184] It can be seen from Examples 1 to 10 and Table 1 that the steel obtained by processing with the technical solution of the present application has a lower oxygen content and a lower impurity content and is of better quality.
[0185] And it can be seen from Table 1 that the comprehensive performance of the steel prepared in Example 3 and Example 8 is better. Therefore, it can be seen that in the technical solution of this application, CaO and SiO 2 When the weight ratio is 3, the comprehensive performance of the prepared steel is better.
[0186] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for improving the purity of molten steel based on slag composition control, characterized in that: The following steps are involved: S1. Optimize slag composition Adjust the ratio of CaO, SiO2, Al2O3 and MgO in the slag; S2. Control the basicity of slag Adjust the weight ratio of CaO to SiO2; S3, add deoxidizer: Add deoxidizer before tapping; S4, Refining Refining technology is used to reduce the gas content in the molten steel and promote the floating of inclusions; the molten steel is stirred to accelerate the reaction between the inclusions and slag and the removal of inclusions.
2. The method for improving the purity of molten steel based on slag composition control according to claim 1, characterized in that: In S1, the CaO, SiO2, Al2O3 and MgO are respectively in parts by weight: 40 to 60 parts of CaO, 13 to 20 parts of SiO2, 5 to 15 parts of Al2O3 and 5 to 20 parts of MgO.
3. The method for improving the purity of molten steel based on slag composition control according to claim 1, characterized in that: In the S2, the weight ratio of CaO to SiO2 is 2.0 to 4.
6.
4. The method for improving the purity of molten steel based on slag composition control according to claim 1, characterized in that: In the S2, the weight ratio of CaO to SiO2 is 3.
5. The method for improving the purity of molten steel based on slag composition control according to claim 1, characterized in that: The deoxidizer is aluminum or ferrosilicon.
6. The method for improving the purity of molten steel based on slag composition control according to claim 1, characterized in that: The refining technology adopts: vacuum degassing (VD) and vacuum argon blowing (RH).
7. The method for improving the purity of molten steel based on slag composition control according to claim 1, characterized in that: The stirring method adopts: ladle argon blowing (SLF) or top argon blowing (TBF).