Method for retarding ring formation of alkaline pellets produced by chain grate-rotary kiln

By adjusting the refractory material composition of the chain grate-rotary kiln production line, the problem of easy ring formation in the production of alkaline pellets by the chain grate-rotary kiln was solved, the production cycle was extended, the production efficiency was improved, and continuous production was achieved.

CN119040623AActive Publication Date: 2024-11-29SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410965935.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-29
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

When producing alkaline pellets using the chain grate-rotary kiln process, the rotary kiln is prone to ring formation, resulting in short production cycles, frequent kiln shutdowns, and reduced production efficiency.

Method used

Adjust the refractory material of the rotary kiln in the chain grate-rotary kiln production line, changing it from Al2O3 and SiO2 as the main components to MgO and Cr2O3 as the main components, and control the refractory material composition as follows: MgO>50%, Cr2O3>20%, SiO2<3%, (K2O+Na2O)<0.5%.

Benefits of technology

It extends the production cycle of alkaline pellets, reduces the frequency of downtime caused by ring formation in rotary kilns, improves production efficiency, and enables continuous production of chain grate-rotary kiln.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for retarding ring formation of alkaline pellets produced by a chain grate-rotary kiln. The method comprises the following steps: weighing and proportioning 70-100 parts of limestone powder, 890-920 parts of iron ore powder and 10 parts of bentonite; uniformly mixing the limestone powder, the iron ore powder and the bentonite through a mixer, and adding the mixture into a disc pelletizer for water replenishing and pelletizing; distributing, drying and preheating the pellets on chain grate-rotary kiln roasting equipment to obtain preheated pellets; the preheated pellets are discharged from the machine head of the chain grate machine and then enter the rotary kiln, high-temperature roasting is continued, and finished pellets are obtained, 50%, Cr2O3 < gt >; 20%, SiO2 1t; 3%, (K2O + Na2O) lt; and 0.5%. According to the invention, the refractory material of the rotary kiln is adjusted from Al2O3 and SiO2 as main components to MgO and Cr2O3 as main components, so that the formation speed of ring-forming substances is slowed down, and the production efficiency of alkaline pellets is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alkaline pellet production, and more specifically relates to a method for slowing down ring formation in alkaline pellet production by a chain grate machine-rotary kiln. Background Art

[0002] Alkaline pellets have good reducing properties and are high-quality raw materials for blast furnaces. Most domestic and foreign companies mainly use belt roasting machine technology to produce alkaline pellets. Its main features are large production capacity of single equipment, high production efficiency, and no problem of easy ring formation in rotary kilns. However, due to the large amount of high-temperature heat-resistant steel used in the equipment, the investment is relatively high, and gas fuel is required. For companies without cheap gas sources, the production and operation costs will be high. Therefore, some companies use chain grate machine-rotary kiln technology to produce alkaline pellets. Its main features are relatively low investment, and coal powder can be used as fuel, and the production and operation costs are low. However, the biggest problem is that the rotary kiln is prone to ring formation when producing alkaline pellets, especially when the SiO2 content of the iron ore powder used is high, it is difficult to produce high-alkalinity alkaline pellets. When the chain grate machine-rotary kiln process is used to produce acidic pellets, the ring formation cycle of the rotary kiln can reach 50 to 60 days, that is, the rotary kiln only needs to deal with the ring formation once after 50 to 60 days of continuous production; but when the chain grate machine-rotary kiln process is used to produce alkaline pellets, the ring formation cycle of the rotary kiln is only 20 to 25 days, and the production cycle is short, which is half of the production cycle of acidic pellets. Therefore, the kiln has to be stopped frequently during the production process to deal with the ring formation, which seriously affects the production efficiency of alkaline pellets. Summary of the invention

[0003] In order to solve the technical problems existing in the above-mentioned prior art, the present invention provides a method for slowing down the ring formation of basic pellets produced by a chain grate machine-rotary kiln, comprising the following steps:

[0004] (1) Ingredients

[0005] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 70-100 parts of limestone powder, 890-920 parts of iron ore powder and 10 parts of bentonite;

[0006] (2) Mixing and pelletizing

[0007] The limestone powder, iron ore powder and bentonite are mixed in a mixer, and then added into a disc pelletizing machine to make pellets by adding water to produce pellets;

[0008] (3) Preheating

[0009] The pellets are distributed, dried and preheated on the grate-rotary kiln roasting equipment to obtain preheated pellets;

[0010] (4) Calcination

[0011] After the preheated pellets come out of the head of the chain grate machine, they enter the rotary kiln and continue to be calcined at high temperature to obtain finished pellets. The temperature of the rotary kiln head is controlled at 1160-1180°C, the hot air temperature of the rotary kiln tail is controlled at 900-950°C, and the refractory material composition of the rotary kiln is controlled as follows: MgO>50%, Cr2O3>20%, SiO2<3%, (K2O+Na2O)<0.5%.

[0012] Furthermore, in the above-mentioned method for slowing down the ring formation of basic pellets produced by chain grate-rotary kiln, the iron grade of the iron ore powder is 65.2%, the SiO2 content is 4.5%; and the CaO content in the limestone powder is 52.4%.

[0013] Furthermore, in the above-mentioned method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln, the moisture content of the pellets obtained by mixing and pelletizing is 9.8% by weight, and the average particle size of the pellets is controlled to be 8-16 mm.

[0014] Furthermore, in the above method for slowing down ring formation of alkaline pellets produced by chain grate-rotary kiln, the binary basicity of the finished alkaline pellets is 1.1.

[0015] As a specific implementation method, in the above-mentioned method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln, the main components of the rotary kiln refractory material are controlled as follows: MgO=51.3%, Cr2O3=20.7%, SiO2=2.8%, (K2O+Na2O)=0.45%.

[0016] As a specific implementation method, in the above-mentioned method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln, the main components of the rotary kiln refractory material are controlled as follows: MgO=54.2%, Cr2O3=20.7%, SiO2=2.8%, (K2O+Na2O)=0.45%.

[0017] As a specific implementation method, in the above-mentioned method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln, the main components of the rotary kiln refractory material are controlled as follows: MgO=57.3%, Cr2O3=20.7%, SiO2=2.8%, (K2O+Na2O)=0.45%.

[0018] As a specific implementation method, in the above-mentioned method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln, the main components of the rotary kiln refractory material are controlled as follows: MgO=51.3%, Cr2O3=23.5%, SiO2=2.8%, (K2O+Na2O)=0.45%.

[0019] As a specific implementation method, in the above-mentioned method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln, the main components of the rotary kiln refractory material are controlled as follows: MgO=51.3%, Cr2O3=26.7%, SiO2=2.8%, (K2O+Na2O)=0.45%.

[0020] As a specific implementation method, in the above-mentioned method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln, the main components of the rotary kiln refractory material are controlled as follows: MgO=51.3%, Cr2O3=28.2%, SiO2=2.8%, (K2O+Na2O)=0.45%.

[0021] The method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln of the present invention has the following advantages and beneficial effects:

[0022] The present invention adjusts the refractory material of the rotary kiln of the chain grate-rotary kiln production line from Al2O3 and SiO2 as main components to MgO and Cr2O3 as main components, thereby slowing down the formation speed of ringing materials in the process of producing alkaline pellets by the chain grate-rotary kiln, and extending the production cycle of the chain grate-rotary kiln in producing alkaline pellets to an average of more than 30 days, thereby significantly reducing the frequency of shutdowns caused by rotary kiln ringing, effectively improving the production efficiency of alkaline pellets, providing strong technical support for realizing the continuous production of alkaline pellets by the chain grate-rotary kiln, and having good promotion value and economic benefits. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] The purpose of the present invention is to slow down the ring formation of alkaline pellets produced by chain grate-rotary kiln, so as to effectively improve the production efficiency of the chain grate-rotary kiln production line, reduce the frequency of shutdown caused by ring formation of rotary kiln, and ensure the smooth production of alkaline pellets. To this end, the present invention provides a method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln. The main technical idea is to adjust the refractory material of the rotary kiln of the chain grate-rotary kiln production line from Al2O3 and SiO2 as the main components to MgO and Cr2O3 as the main components. Through this technical measure, the formation speed of rings in the process of chain grate-rotary kiln production of alkaline pellets can be effectively slowed down, solving the problem of ring formation in the production of alkaline pellets by chain grate-rotary kiln, which is conducive to improving the production efficiency of alkaline pellets.

[0025] Specifically, the method for slowing down the ring formation of basic pellets produced by a chain grate machine-rotary kiln of the present invention comprises the following steps:

[0026] (1) Ingredients

[0027] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 70-100 parts of limestone powder, 890-920 parts of iron ore powder and 10 parts of bentonite, wherein the iron ore powder is iron ore powder from Lan County, Shanxi Province, with an iron grade of 65.2% and a SiO2 content of 4.5%, the CaO content in the limestone powder is 52.4%, and the bentonite is conventional bentonite purchased from the market.

[0028] (2) Mixing and pelletizing

[0029] The limestone powder, iron ore powder and bentonite are mixed in a mixer, and then added into a disc pelletizing machine to make pellets with a moisture content of 9.8% by weight. The average particle size of the pellets is controlled to be 8-16 mm.

[0030] (3) Preheating

[0031] The pellets are distributed, dried and preheated on the chain grate-rotary kiln roasting equipment to obtain preheated pellets.

[0032] (4) Calcination

[0033] The preheated pellets come out of the head of the chain grate machine and enter the rotary kiln for continued high-temperature roasting to obtain finished pellets, wherein the temperature of the rotary kiln head is controlled at 1160-1180°C, the hot air temperature of the rotary kiln tail is controlled at 900-950°C, the binary basicity (CaO / SiO2) of the finished pellet ore is controlled at 1.1, and the refractory material composition of the rotary kiln is controlled as follows: MgO>50%, Cr2O3>20%, SiO2<3%, (K2O+Na2O)<0.5%.

[0034] The method for alleviating ring formation in the production of alkaline pellets by a chain grate machine-rotary kiln of the present invention is further described below in combination with the reference embodiment in the prior art and the embodiments of the present invention.

[0035] Benchmark Example

[0036] The benchmark example is a conventional method for producing alkaline pellets using a chain grate-rotary kiln process, and the specific production steps are as follows:

[0037] (1) Ingredients

[0038] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 94 parts of limestone powder, 896 parts of iron ore powder and 10 parts of bentonite, wherein the iron ore powder is iron ore powder from Lan County, Shanxi Province, with an iron grade of 65.2% and a SiO2 content of 4.5%. The CaO content in the limestone powder is 52.4%, and the bentonite is conventional bentonite purchased from the market.

[0039] (2) Mixing and pelletizing

[0040] The limestone powder, iron ore powder and bentonite are mixed evenly in a mixer, and then added into a disc pelletizing machine and supplemented with water to produce pellets with a moisture content of 9.8% by weight and an average particle size of 8 to 16 mm.

[0041] (3) Preheating

[0042] The pellets are distributed, dried and preheated on the chain grate-rotary kiln roasting equipment to obtain preheated pellets.

[0043] (4) Calcination

[0044] After the preheated pellets come out of the head of the chain grate machine, they enter the rotary kiln and continue to be calcined at high temperature to obtain finished pellets. The temperature of the rotary kiln head is 1160-1180°C, the hot air temperature of the rotary kiln tail is 900-950°C, the binary basicity of the finished pellet ore is 1.1, and the main components of the rotary kiln refractory material are: Al2O3=78.3%, SiO2=15%, CaO=1.1%, (K2O+Na2O)=0.68%.

[0045] According to actual calculation, in the benchmark example, the kiln needs to be stopped for processing the rings in the kiln after an average of 23 days of production. The above benchmark example shows that when roasting alkaline pellets, the rotary kiln is prone to ring formation, and the kiln needs to be stopped for processing the rings in the kiln after an average of about 23 days of production. The formation speed of the rings is fast and the production cycle is short, resulting in low production efficiency of alkaline pellets produced by conventional process methods using chain grate machine-rotary kiln.

[0046] Example 1

[0047] In Example 1 of the present invention, the refractory material of the rotary kiln of the chain grate-rotary kiln production line is adjusted from Al2O3 and SiO2 as the main components to MgO and Cr2O3 as the main components. Specifically, the method for slowing down the ring formation of basic pellets produced by the chain grate-rotary kiln of Example 1 comprises the following steps:

[0048] (1) Ingredients

[0049] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 94 parts of limestone powder, 896 parts of iron ore powder and 10 parts of bentonite, wherein the iron ore powder is iron ore powder from Lan County, Shanxi Province, with an iron grade of 65.2% and a SiO2 content of 4.5%. The CaO content in the limestone powder is 52.4%, and the bentonite is conventional bentonite purchased from the market.

[0050] (2) Mixing and pelletizing

[0051] The limestone powder, iron ore powder and bentonite are mixed evenly in a mixer, and then added into a disc pelletizing machine to make pellets with a moisture content of 9.8% by weight and an average particle size of 8 to 16 mm.

[0052] (3) Preheating

[0053] The pellets are distributed, dried and preheated on the chain grate-rotary kiln roasting equipment to obtain preheated pellets.

[0054] (4) Calcination

[0055] The preheated pellets come out of the head of the chain grate machine and enter the rotary kiln for continued high-temperature roasting to obtain finished pellets. The temperature of the rotary kiln head is 1160-1180°C, the hot air temperature of the rotary kiln tail is 900-950°C, the binary basicity of the finished pellet ore is 1.1, and the main components of the rotary kiln refractory material are: MgO = 51.3%, Cr2O3 = 20.7%, SiO2 = 2.8%, (K2O + Na2O) = 0.45%.

[0056] According to actual calculation, in Example 1 of the present invention, the kiln needs to be stopped for processing the rings in the kiln after an average of 29 days of production. The above Example 1 shows that by using new refractory materials to replace the original refractory materials, the kiln needs to be stopped for processing the rings in the kiln after an average of about 29 days of production. Compared with the benchmark example in the prior art, the production cycle of the chain grate-rotary kiln for producing alkaline pellets is extended by 6 days, which effectively improves the production efficiency of alkaline pellets.

[0057] Example 2

[0058] In Example 2 of the present invention, the MgO content ratio in the refractory material of the rotary kiln of the chain grate-rotary kiln production line is increased from 51.3% in Example 1 to 54.2%, and the contents of the other main components Cr2O3, SiO2 and K2O+Na2O are the same as those in Example 1. Specifically, the method for slowing down the ring formation of basic pellets produced by the chain grate-rotary kiln in Example 2 comprises the following steps:

[0059] (1) Ingredients

[0060] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 94 parts of limestone powder, 896 parts of iron ore powder and 10 parts of bentonite, wherein the iron ore powder is iron ore powder from Lan County, Shanxi Province, with an iron grade of 65.2% and a SiO2 content of 4.5%. The CaO content in the limestone powder is 52.4%, and the bentonite is conventional bentonite purchased from the market.

[0061] (2) Mixing and pelletizing

[0062] The limestone powder, iron ore powder and bentonite are mixed evenly in a mixer, and then added into a disc pelletizing machine to make pellets with a moisture content of 9.8% by weight and an average particle size of 8 to 16 mm.

[0063] (3) Preheating

[0064] The pellets are distributed, dried and preheated on the chain grate-rotary kiln roasting equipment to obtain preheated pellets.

[0065] (4) Calcination

[0066] After the preheated pellets come out of the head of the chain grate machine, they enter the rotary kiln and continue to be calcined at high temperature to obtain finished pellets. The temperature of the rotary kiln head is 1160-1180°C, the hot air temperature of the rotary kiln tail is 900-950°C, the binary basicity of the finished pellet ore is 1.1, and the main components of the rotary kiln refractory material are: MgO = 54.2%, Cr2O3 = 20.7%, SiO2 = 2.8%, (K2O + Na2O) = 0.45%.

[0067] According to actual calculation, in Example 2 of the present invention, the kiln needs to be stopped for 30 days of production on average to treat the rings in the kiln. The above Example 2 shows that by increasing the MgO content in the refractory material from 51.3% in Example 1 to 54.2%, the production cycle of the chain grate-rotary kiln for producing alkaline pellets is extended by 1 day compared with Example 1, and extended by 7 days compared with the benchmark example in the prior art, effectively improving the production efficiency of alkaline pellets.

[0068] Example 3

[0069] In Example 3 of the present invention, the MgO content ratio in the refractory material of the rotary kiln of the chain grate-rotary kiln production line is increased from 54.2% in Example 2 to 57.3%, and the contents of the other main components Cr2O3, SiO2 and K2O+Na2O are the same as those in Example 2. Specifically, the method for slowing down the ring formation of basic pellets produced by the chain grate-rotary kiln in Example 3 comprises the following steps:

[0070] (1) Ingredients

[0071] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 94 parts of limestone powder, 896 parts of iron ore powder and 10 parts of bentonite, wherein the iron ore powder is iron ore powder from Lan County, Shanxi Province, with an iron grade of 65.2% and a SiO2 content of 4.5%. The CaO content in the limestone powder is 52.4%, and the bentonite is conventional bentonite purchased from the market.

[0072] (2) Mixing and pelletizing

[0073] The limestone powder, iron ore powder and bentonite are mixed evenly in a mixer, and then added into a disc pelletizing machine to make pellets with a moisture content of 9.8% by weight and an average particle size of 8 to 16 mm.

[0074] (3) Preheating

[0075] The pellets are distributed, dried and preheated on the chain grate-rotary kiln roasting equipment to obtain preheated pellets.

[0076] (4) Calcination

[0077] After the preheated pellets come out of the head of the chain grate machine, they enter the rotary kiln and continue to be calcined at high temperature to obtain finished pellets. The temperature of the rotary kiln head is 1160-1180°C, the hot air temperature of the rotary kiln tail is 900-950°C, the binary basicity of the finished pellet ore is 1.1, and the main components of the rotary kiln refractory material are: MgO = 57.3%, Cr2O3 = 20.7%, SiO2 = 2.8%, (K2O + Na2O) = 0.45%.

[0078] According to actual measurement, in Example 3 of the present invention, the kiln needs to be stopped for processing the rings in the kiln after an average of 30.5 days of production. The above Example 3 shows that by increasing the MgO content in the refractory material from 54.2% in Example 2 to 57.3%, the production cycle of the chain grate-rotary kiln for producing alkaline pellets is extended by 0.5 days compared with Example 2, and extended by 7.5 days compared with the benchmark example in the prior art, effectively improving the production efficiency of alkaline pellets.

[0079] Example 4

[0080] In Example 4 of the present invention, the content of Cr2O3 in the refractory material of the rotary kiln of the chain grate-rotary kiln production line is increased from 20.7% in Example 1 to 23.5%, and the contents of the other main components MgO, SiO2 and K2O+Na2O are the same as those in Example 1. Specifically, the method for slowing down the ring formation of basic pellets produced by the chain grate-rotary kiln of Example 4 comprises the following steps:

[0081] (1) Ingredients

[0082] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 94 parts of limestone powder, 896 parts of iron ore powder and 10 parts of bentonite, wherein the iron ore powder is iron ore powder from Lan County, Shanxi Province, with an iron grade of 65.2% and a SiO2 content of 4.5%. The CaO content in the limestone powder is 52.4%, and the bentonite is conventional bentonite purchased from the market.

[0083] (2) Mixing and pelletizing

[0084] The limestone powder, iron ore powder and bentonite are mixed evenly in a mixer, and then added into a disc pelletizing machine to make pellets with a moisture content of 9.8% by weight and an average particle size of 8 to 16 mm.

[0085] (3) Preheating

[0086] The pellets are distributed, dried and preheated on the chain grate-rotary kiln roasting equipment to obtain preheated pellets.

[0087] (4) Calcination

[0088] The preheated pellets come out of the grate machine head and enter the rotary kiln, where they continue high-temperature roasting to obtain finished pellets. The temperature at the rotary kiln head is 1160-1180°C, the hot air temperature at the rotary kiln tail is 900-950°C, the binary basicity of the finished pellet ore is 1.1, and the main components of the rotary kiln refractory material are: MgO = 51.3%, Cr2O3 = 23.5%, SiO2 = 2.8%, (K2O + Na2O) = 0.45%.

[0089] According to actual calculation, in Example 4 of the present invention, the kiln needs to be stopped for 31 days on average to treat the ringed materials in the kiln. The above Example 4 shows that by increasing the Cr2O3 content in the refractory material from 20.7% in Example 1 to 23.5%, the production cycle of the chain grate-rotary kiln for producing alkaline pellets is extended by 2 days compared with Example 1, and by 8 days compared with the benchmark example in the prior art, which effectively improves the production efficiency of alkaline pellets.

[0090] Example 5

[0091] In Example 5 of the present invention, the content ratio of Cr2O3 in the refractory material of the rotary kiln of the chain grate-rotary kiln production line is increased from 23.5% in Example 4 to 26.7%, and the contents of the other main components MgO, SiO2 and K2O+Na2O are the same as those in Example 4. Specifically, the method for slowing down the ring formation of basic pellets produced by the chain grate-rotary kiln in Example 5 comprises the following steps:

[0092] (1) Ingredients

[0093] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 94 parts of limestone powder, 896 parts of iron ore powder and 10 parts of bentonite, wherein the iron ore powder is iron ore powder from Lan County, Shanxi Province, with an iron grade of 65.2% and a SiO2 content of 4.5%. The CaO content in the limestone powder is 52.4%, and the bentonite is conventional bentonite purchased from the market.

[0094] (2) Mixing and pelletizing

[0095] The limestone powder, iron ore powder and bentonite are mixed evenly in a mixer, and then added into a disc pelletizing machine to make pellets with a moisture content of 9.8% by weight and an average particle size of 8 to 16 mm.

[0096] (3) Preheating

[0097] The pellets are distributed, dried and preheated on the chain grate-rotary kiln roasting equipment to obtain preheated pellets.

[0098] (4) Calcination

[0099] After the preheated pellets come out of the head of the chain grate machine, they enter the rotary kiln and continue to be calcined at high temperature to obtain finished pellets. The temperature of the rotary kiln head is 1160-1180°C, the hot air temperature of the rotary kiln tail is 900-950°C, the binary basicity of the finished pellet ore is 1.1, and the main components of the rotary kiln refractory material are: MgO = 51.3%, Cr2O3 = 26.7%, SiO2 = 2.8%, (K2O + Na2O) = 0.45%.

[0100] According to actual calculation, in Example 5 of the present invention, the kiln needs to be stopped for an average of 32 days of production to treat the ringed materials in the kiln. The above Example 5 shows that by increasing the Cr2O3 content ratio in the refractory material from 23.5% in Example 4 to 26.7%, the production cycle of the chain grate-rotary kiln for producing alkaline pellets is extended by 1 day compared with Example 4, and extended by 9 days compared with the benchmark example in the prior art, effectively improving the production efficiency of alkaline pellets.

[0101] Example 6

[0102] In Example 6 of the present invention, the content ratio of Cr2O3 in the refractory material of the rotary kiln of the chain grate-rotary kiln production line is increased from 26.7% in Example 4 to 28.2%, and the contents of the other main components MgO, SiO2 and K2O+Na2O are the same as those in Example 5. Specifically, the method for slowing down the ring formation of basic pellets produced by the chain grate-rotary kiln of Example 6 comprises the following steps:

[0103] (1) Ingredients

[0104] Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 94 parts of limestone powder, 896 parts of iron ore powder and 10 parts of bentonite, wherein the iron ore powder is iron ore powder from Lan County, Shanxi Province, with an iron grade of 65.2% and a SiO2 content of 4.5%. The CaO content in the limestone powder is 52.4%, and the bentonite is conventional bentonite purchased from the market.

[0105] (2) Mixing and pelletizing

[0106] The limestone powder, iron ore powder and bentonite are mixed evenly in a mixer, and then added into a disc pelletizing machine to make pellets with a moisture content of 9.8% by weight and an average particle size of 8 to 16 mm.

[0107] (3) Preheating

[0108] The pellets are distributed, dried and preheated on the chain grate-rotary kiln roasting equipment to obtain preheated pellets.

[0109] (4) Calcination

[0110] After the preheated pellets come out of the head of the chain grate machine, they enter the rotary kiln and continue to be calcined at high temperature to obtain finished pellets. The temperature of the rotary kiln head is 1160-1180°C, the hot air temperature of the rotary kiln tail is 900-950°C, the binary basicity of the finished pellet ore is 1.1, and the main components of the rotary kiln refractory material are: MgO = 51.3%, Cr2O3 = 28.2%, SiO2 = 2.8%, (K2O + Na2O) = 0.45%.

[0111] According to actual calculation, in Example 6 of the present invention, the kiln needs to be stopped for processing the rings in the kiln after an average of 32.5 days of production. The above Example 6 shows that by increasing the Cr2O3 content in the refractory material from 26.7% in Example 5 to 28.2%, the production cycle of the chain grate-rotary kiln for producing alkaline pellets is extended by 0.5 days compared with Example 5, and extended by 9.5 days compared with the benchmark example in the prior art, effectively improving the production efficiency of alkaline pellets.

[0112] In summary, the method for slowing down the ring formation of alkaline pellets produced by a chain grate-rotary kiln of the present invention adjusts the refractory material of the rotary kiln of the chain grate-rotary kiln production line from Al2O3 and SiO2 as the main components to MgO and Cr2O3 as the main components, thereby slowing down the formation rate of rings in the process of producing alkaline pellets by the chain grate-rotary kiln, and extending the production cycle of alkaline pellets produced by the chain grate-rotary kiln to an average of more than 30 days. That is, by utilizing the method for slowing down the ring formation of alkaline pellets produced by a chain grate-rotary kiln of the present invention, it is possible to achieve an average of 30 days of production before the kiln needs to be stopped to treat the rings in the kiln, which is extended by more than 7 days compared with the prior art, thereby significantly reducing the frequency of shutdowns caused by ring formation in the rotary kiln, effectively improving the production efficiency of alkaline pellets, and providing strong technical support for realizing continuous production of alkaline pellets by a chain grate-rotary kiln, and having good promotion value and economic benefits.

[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features therein may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the present invention.

Claims

1. A method for slowing down the ring formation of alkaline pellets produced by chain grate-rotary kiln, It is characterized in that The following steps are involved: (1) Ingredients Iron ore powder, limestone powder and bentonite are weighed and mixed according to the following weight proportions: 70-100 parts of limestone powder, 890-920 parts of iron ore powder and 10 parts of bentonite; (2) Mixing and pelletizing The limestone powder, iron ore powder and bentonite are mixed in a mixer, and then added into a disc pelletizing machine to make pellets by adding water to produce pellets; (3) Preheating The pellets are distributed, dried and preheated on the grate-rotary kiln roasting equipment to obtain preheated pellets; (4) Calcination After the preheated pellets come out of the grate machine head, they enter the rotary kiln and continue to be roasted at high temperature to obtain finished pellets. The temperature of the rotary kiln head is controlled at 1160-1180℃, the hot air temperature of the rotary kiln tail is controlled at 900-950℃, and the refractory material composition of the rotary kiln is controlled as follows: MgO>50%, Cr 2 O 3 >20%、SiO 2 <3%、(K 2 O+Na 2 O)<0.5%.

2. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The iron grade of iron ore powder is 65.2%, SiO 2 The content is 4.5%; the CaO content in limestone powder is 52.4%.

3. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The moisture content of the pellets obtained by mixing and pelletizing is 9.8% by weight, and the average particle size of the pellets is controlled to be 8-16 mm.

4. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The binary basicity of the finished alkaline pellets is 1.

1.

5. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The main components of the rotary kiln refractory material are controlled as follows: MgO = 51.3%, Cr 2 O 3 =20.7%, SiO 2 =2.8%, (K 2 O+Na 2 O)=0.45%.

6. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The main components of the rotary kiln refractory material are controlled as follows: MgO = 54.2%, Cr 2 O 3 =20.7%, SiO 2 =2.8%, (K 2 O+Na 2 O)=0.45%.

7. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The main components of the rotary kiln refractory material are controlled as follows: MgO = 57.3%, Cr 2 O 3 =20.7%, SiO 2 =2.8%, (K 2 O+Na 2 O)=0.45%.

8. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The main components of the rotary kiln refractory material are controlled as follows: MgO = 51.3%, Cr 2 O 3 =23.5%, SiO 2 =2.8%, (K 2 O+Na 2 O)=0.45%.

9. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The main components of the rotary kiln refractory material are controlled as follows: MgO = 51.3%, Cr 2 O 3 =26.7%, SiO 2 =2.8%, (K 2 O+Na 2 O)=0.45%.

10. The method for slowing down the ring formation of alkaline pellets produced by chain grate machine-rotary kiln according to claim 1, It is characterized in that The main components of the rotary kiln refractory material are controlled as follows: MgO = 51.3%, Cr 2 O 3 =28.2%, SiO 2 =2.8%, (K 2 O+Na 2 O)=0.45%.

Citation Information

Patent Citations

  • Process for producing ss-2caosio2

    CN103328383A

  • Pellet production method for reducing agglomeration proportion of pellets

    CN111676368A

  • Pellet production method for delaying nodulation of rotary kiln

    CN111876591A

  • Preparation method of high-toughness refractory material

    CN112645720A

  • Production method of ring-forming-resistant environment-friendly refractory brick of rotary kiln for preparing sulfuric acid from gypsum