Three-vacuum smelting process for Ni-based aging strengthening type high-temperature alloy GH4698 cast ingot
Through the three-vacuum smelting process, including vacuum induction smelting, annealing and multiple vacuum self-consumption smelting, the composition uniformity and purity of GH4698 ingots are solved, the quality and stability of the ingots are significantly improved, and the risk of metallurgical defects is reduced. .
Patent Information
- Application Number
- CN202411008781.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing dual-connection process of GH4698 ingots has different electrode density, high inclusion content, poor surface quality and high metallurgical defects, making it difficult to obtain high purity, high uniformity, high consistency and high performance ingots.
Three vacuum smelting processes are adopted, including vacuum induction smelting, annealing, first and second vacuum self-consumption smelting, modification and surface treatment. Through melting speed and droplet control, the vacuum degree and leakage rate are ensured within the appropriate range. , gradually improve the composition uniformity and purity of the electrodes and ingots.
The composition uniformity and purity of GH4698 ingots have been improved, which significantly reduces the content, stability and surface quality of impurities, and reduces the risk of metallurgical defects.
Smart Images

Figure CN119040673A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature alloy smelting, and in particular to a triple-vacuum smelting process for a Ni-based aging-strengthened high-temperature alloy GH4698 ingot. Background Art
[0002] GH4698 alloy is a kind of Ni-Cr based deformable high temperature alloy, which is developed on the basis of GH4033 high temperature alloy. By increasing the content of aluminum and titanium alloy and reducing the content of chromium alloy, the high temperature alloy has high endurance strength, good plasticity and comprehensive performance in the range of 600-800℃. With the localization demand for materials for a certain engine turbine disk, the order volume of GH4698 alloy bars is increasing day by day, which puts forward higher requirements on the composition uniformity and inclusion content of GH4698 bars produced by metallurgical plants.
[0003] At present, the GH4698 ingots produced at home and abroad generally adopt the dual process (vacuum induction melting + vacuum consumable melting). The electrodes cast by vacuum induction melting have many internal shrinkage cavities, poor electrode density, high inclusion content, and the risk of cracking of the electrodes, which leads to poor stability in the subsequent consumable melting process, high inclusion content, poor surface quality of the finished ingot, and a high risk of metallurgical defects. More importantly, due to the poor stability of the dual production process, the melting process has limited removal of inclusions and gases, making it difficult to obtain ingots with high purity, high uniformity, high consistency, and high performance. Summary of the invention
[0004] The object of the present invention is to provide a three-vacuum smelting process for Ni-based aging-strengthened high-temperature alloy GH4698 ingot to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a three-vacuum smelting process for a Ni-based aging-strengthened high-temperature alloy GH4698 ingot, comprising the following steps:
[0006] S1: GH4698 alloy VIM electrode obtained by vacuum induction melting (VIM);
[0007] S2: annealing the VIM electrode obtained after S1;
[0008] S3: subjecting the VIM electrode obtained after S2 to the first vacuum consumable melting (VAR) to obtain a GH4648 alloy VAR electrode;
[0009] S4: reforging the VAR electrode obtained after S3 on a fast forging machine;
[0010] S5: After the forged electrode is surface treated, it is placed in an oven for baking.
[0011] S6: The VAR electrode obtained after S4 is subjected to a second vacuum consumable melting (VAR) to obtain a GH4648 alloy ingot.
[0012] Preferably, in S1, the GH4698 alloy VIM electrode has the following chemical compositions by mass percentage: C: 0.040%-0.060%, Cr: 13.50%-14.50%, Mo: 2.90%-3.10%, Nb: 1.80%-2.00%, Ti: 2.40%-2.60%, Al: 1.60%-1.75%, B: 0.0040%-0.0045%, Zr: 0.025%-0.040%, Fe: 0.35%-1.00%, and the rest is Ni, wherein Nb, B and Mo are added in the form of intermediate alloys NiNb, NiB and NiMo, and the sum of the mass percentages of the above components is 100%.
[0013] Preferably, in S2, specifically: placing the GH4698 alloy VIM electrode in a natural gas furnace for heating treatment, the heating temperature is 900°C to 1200°C, the insulation time is 6h to 10h, after the insulation is completed, the natural gas furnace is cooled to 500°C to 600°C, and then air-cooled.
[0014] Preferably, in said S3, the self-consumable stable smelting stage adopts melting speed + droplet control, the melting speed is 4.0-6.0 kg / min, the droplet is 3-121 / s, and the droplet range of droplet control statistics is 2-141 / s. The vacuum degree is ≤0.5 Pa, and the leakage rate is ≤0.5.
[0015] Preferably, in S4, the electrode with a diameter of Φ500 is stretched to Φ450 in all directions, and then rounded to Φ440 (+5, -5), wherein the initial forging temperature is ≥900°C and the final forging temperature is ≥800°C.
[0016] Preferably, in S5, the electrode is subjected to surface grinding after forging, requiring the surface to be free of oxide scale and pores, and then the rotten ends are cut flat. The electrode is baked at a temperature of 100° C. for a time of ≥ 2 hours.
[0017] Preferably, in said S6, the self-consumable stable smelting stage adopts melting speed + droplet control, the melting speed is 3.0-3.8 kg / min, the droplet is 4-81 / s, the melting speed fluctuation range is ≤10%, and the droplet range of droplet control statistics is 3-101 / s. The vacuum degree is ≤0.5 Pa, and the leakage rate is ≤0.5.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1) The GH4698 alloy ingot produced by the triple vacuum smelting process of the present invention has good composition uniformity, and the extreme differences of elements such as C, Cr, Mo, Nb, Ti, Al, Nb, B, Zr, Fe, and Ni are small.
[0020] 2) The GH4698 alloy ingot produced by the triple vacuum smelting process of the present invention has high purity and extremely low content of impurity elements such as O, N, H, S, and P.
[0021] 3) The GH4698 alloy ingot produced by the triple vacuum smelting process of the present invention has a stable smelting process and good surface quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a real picture of Φ500mmGH4698 high-temperature alloy ingot. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] See also Figure 1 The present invention provides a technical solution: a three-vacuum smelting process for the Ni-based aging-strengthened high-temperature alloy GH4698 ingot of the present invention, which is specifically implemented according to the following S:
[0025] S1, a GH4698 alloy VIM electrode with a diameter of 500 (± 2) mm is obtained by vacuum induction melting (VIM), and its chemical composition is as follows by mass percentage: C: 0.040%-0.060%, Cr: 13.50%-14.50%, Mo: 2.90%-3.10%, Nb: 1.80%-2.00%, Ti: 2.40%-2.60%, Al: 1.60%-1.75%, B: 0.0040%-0.0045%, Zr: 0.025%-0.040%, Fe: 0.35%-1.00%, wherein Nb, B, and Mo are added in the form of intermediate alloys NiNb, NiB, and NiMo, and the rest is Ni, and the sum of the mass percentages of the above components is 100%;
[0026] S2, annealing the VIM electrode obtained after S1;
[0027] Specifically, the GH4698 alloy VIM electrode is placed in a natural gas furnace for heating treatment at a temperature of 900°C to 1200°C for a holding time of 6h to 10h. After the holding time is completed, the natural gas furnace is cooled to 500°C to 600°C and then air-cooled.
[0028] S3, the VIM electrode obtained after S2 is subjected to the first vacuum consumable melting (VAR), the melting rate + droplet control is adopted in the consumable stable melting stage, the melting rate is 4.0-6.0kg / min, the droplet is 3-121 / s, and the droplet range of the droplet control statistics is 2-141 / s. The vacuum degree is ≤0.5Pa, the leakage rate is ≤0.5, and the GH4648 alloy VAR electrode with a diameter of 500 (±10) mm is obtained;
[0029] S4: The VAR electrode obtained after S3 is forged on a fast forging machine, and the Ф500 electrode is stretched to Ф450, and then rounded to Ф440 (+5, -5), wherein the initial forging temperature is ≥900°C and the final forging temperature is ≥800°C, to obtain a GH4648 alloy VAR electrode with a diameter of 440 (+5, -5) mm;
[0030] S5: Grind the surface of the electrode after forging in S4, requiring no oxide scale and pores on the surface, and then cut off the rotten ends. Bake the electrode at a temperature of 100℃ for ≥2h.
[0031] S6: The electrode obtained after S5 is subjected to the second vacuum consumable melting (VAR). The consumable stable melting stage adopts melting speed + droplet control, the melting speed is 3.0-3.8kg / min, the droplet is 4-81 / s, the melting speed fluctuation range is ≤10%, and the droplet range of the droplet control statistics is 3-101 / s. The vacuum degree is ≤0.5Pa, and the leakage rate is ≤0.5.
[0032] Example 1
[0033] The three-vacuum smelting process of the Ni-based aging-strengthened high-temperature alloy GH4698 ingot of the present invention is specifically implemented according to the following S:
[0034] S1, a GH4698 alloy VIM electrode with a diameter of 440 mm was obtained by vacuum induction melting (VIM), and its chemical composition by mass percentage was: C: 0.043%, Cr: 14.12%, Mo: 2.96%, Nb: 1.98%, Ti: 2.42%, Al: 1.62%, B: 0.0042%, Zr: 0.028%, Fe: 0.66%, wherein Nb, B, and Mo were added in the form of intermediate alloys NiNb, NiB, and NiMo, and the rest was Ni, and the sum of the mass percentages of the above components was 100%;
[0035] S2, annealing the VIM electrode obtained after S1;
[0036] Specifically, the GH4698 alloy VIM electrode is placed in a natural gas furnace for heating treatment at a temperature of 1000°C and a holding time of 8 hours. After the holding time is completed, the natural gas furnace is cooled to 580°C and then air-cooled.
[0037] S3, the VIM electrode obtained after S2 is subjected to the first vacuum consumable melting (VAR), and the melting rate + droplet control is adopted in the consumable stable melting stage, the melting rate is 5.5kg / min, the droplet is 101 / s, the vacuum degree is 0.09Pa, the leakage rate is 0.083, and the GH4648 alloy VAR electrode with a diameter of 498mm is obtained;
[0038] S4: The VAR electrode obtained after S3 is forged on a fast forging machine, and the Ф498 specification electrode is stretched to Ф450 in all directions, and then rounded to Ф440 (+5, -5), wherein the initial forging temperature is 989°C and the final forging temperature is 868°C, and a GH4648 alloy VAR electrode with a diameter of 443 mm is obtained;
[0039] S5: Grind the surface of the electrode after forging in S4, and then cut off the rotten ends. Bake the electrode at a temperature of 100°C for 4 hours;
[0040] S6: The electrode obtained after S5 was subjected to the second vacuum consumable melting (VAR). The consumable stable melting stage adopted the melting rate + droplet control, the melting rate was 3.15kg / min, the droplet was 51 / s, the process was stable without melting rate fluctuation. The vacuum degree was 0.076Pa, and the leakage rate was 0.089. A GH4648 alloy ingot with a diameter of 496mm was obtained.
[0041] Samples were taken at the head and tail of the ingot for composition testing, and the results are shown in Table 1.
[0042] Table 1 GH4698 alloy ingot composition
[0043]
[0044] Example 2
[0045] The three-vacuum smelting process of the Ni-based aging-strengthened high-temperature alloy GH4698 ingot of the present invention is specifically implemented according to the following S:
[0046] S1, a GH4698 alloy VIM electrode with a diameter of 440 mm was obtained by vacuum induction melting (VIM), and its chemical composition by mass percentage was: C: 0.046%, Cr: 14.32%, Mo: 2.91%, Nb: 1.89%, Ti: 2.52%, Al: 1.70%, B: 0.0043%, Zr: 0.032%, Fe: 0.41%, wherein Nb, B, and Mo were added in the form of intermediate alloys NiNb, NiB, and NiMo, and the rest was Ni, and the sum of the mass percentages of the above components was 100%;
[0047] S2, annealing the VIM electrode obtained after S1;
[0048] Specifically, the GH4698 alloy VIM electrode is placed in a natural gas furnace for heating treatment at a temperature of 1000°C and a holding time of 8 hours. After the holding time is completed, the natural gas furnace is cooled to 580°C and then air-cooled.
[0049] S3, the VIM electrode obtained after S2 is subjected to the first vacuum consumable melting (VAR), and the melting rate + droplet control is adopted in the consumable stable melting stage, the melting rate is 4.5kg / min, the droplet is 101 / s, the vacuum degree is 0.106Pa, the leakage rate is 0.097, and the GH4648 alloy VAR electrode with a diameter of 498mm is obtained;
[0050] S4: The VAR electrode obtained after S3 is forged on a fast forging machine, and the Ф498 specification electrode is stretched to Ф450 in all directions, and then rounded to Ф440 (+5, -5), wherein the initial forging temperature is 976°C and the final forging temperature is 845°C, and a GH4648 alloy VAR electrode with a diameter of 441 mm is obtained;
[0051] S5: Grind the surface of the electrode after forging in S4, and then cut off the rotten ends. Bake the electrode at a temperature of 100°C for 4 hours;
[0052] S6: The electrode obtained after S5 was subjected to the second vacuum consumable melting (VAR). The consumable stable melting stage adopted the melting rate + droplet control, the melting rate was 3.75kg / min, the droplet was 51 / s, the process was stable without melting rate fluctuation. The vacuum degree was 0.081Pa, and the leakage rate was 0.064. A GH4648 alloy ingot with a diameter of 497mm was obtained.
[0053] Samples were taken at the head and tail of the ingot for composition testing, and the results are shown in Table 2.
[0054] Table 2 GH4698 alloy ingot composition
[0055]
[0056] After two vacuum self-consumable remeltings, the extreme difference between the main elements and trace elements in the ingot is small, and the composition uniformity is good. The average content of harmful elements S in the ingot is about 6ppm, the content of P is about 40ppm, the content of gaseous elements O is about 5ppm, and the content of H reaches the lower limit of the test.
[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A three-vacuum smelting process for Ni-based aging-strengthened high-temperature alloy GH4698 ingot, characterized in that: Includes steps: S1: GH4698 alloy VIM electrode obtained by vacuum induction melting (VIM); S2: annealing the VIM electrode obtained after S1; S3: subjecting the VIM electrode obtained after S2 to the first vacuum consumable melting (VAR) to obtain a GH4648 alloy VAR electrode; S4: reforging the VAR electrode obtained after S3 on a fast forging machine; S5: After the forged electrode is surface treated, it is placed in an oven for baking. S6: The VAR electrode obtained after S4 is subjected to a second vacuum consumable melting (VAR) to obtain a GH4648 alloy ingot.
2. The triple vacuum smelting process for the Ni-based aging-hardened high-temperature alloy GH4698 ingot according to claim 1 is characterized in that: The GH4698 alloy VIM electrode in S1 has the following chemical compositions by mass percentage: C: 0.040%-0.060%, Cr: 13.50%-14.50%, Mo: 2.90%-3.10%, Nb: 1.80%-2.00%, Ti: 2.40%-2.60%, Al: 1.60%-1.75%, B: 0.0040%-0.0045%, Zr: 0.025%-0.040%, Fe: 0.35%-1.00%, and the rest is Ni, wherein Nb, B, and Mo are added in the form of intermediate alloys NiNb, NiB, and NiMo, and the sum of the mass percentages of the above components is 100%.
3. The triple vacuum smelting process for the Ni-based aging-hardened high-temperature alloy GH4698 ingot according to claim 1 is characterized in that: The specific method in S2 is: placing the GH4698 alloy VIM electrode in a natural gas furnace for heating treatment, the heating temperature is 900°C to 1200°C, the insulation time is 6h to 10h, after the insulation is completed, the natural gas furnace is cooled to 500°C to 600°C, and then air-cooled.
4. The triple vacuum smelting process for the Ni-based aging-hardened high-temperature alloy GH4698 ingot according to claim 1 is characterized in that: The self-consumable stable melting stage in S3 adopts melting speed + droplet control, the melting speed is 4.0-6.0kg / min, the droplet is 3-121 / s, and the droplet range of droplet control statistics is 2-141 / s. The vacuum degree is ≤0.5Pa, and the leakage rate is ≤0.
5.
5. The triple vacuum smelting process for the Ni-based aging-hardened high-temperature alloy GH4698 ingot according to claim 1 is characterized in that: The method of S4 is to draw the Ф500 specification electrode into eight directions to Ф450, and then round it to Ф440 (+5, -5), wherein the initial forging temperature is ≥900°C and the final forging temperature is ≥800°C.
6. The triple vacuum smelting process for the Ni-based aging-hardened high-temperature alloy GH4698 ingot according to claim 1 is characterized in that: After the forging in S5, the electrode is subjected to surface grinding treatment, requiring the surface to be free of oxide scale and pores, and then the rotten ends are cut flat. The electrode is baked at a temperature of 100° C. for a time of ≥ 2 hours.
7. The triple vacuum smelting process for the Ni-based aging-hardened high-temperature alloy GH4698 ingot according to claim 1 is characterized in that: The self-consumable stable smelting stage in S6 adopts melting speed + molten drop control, the melting speed is 3.0-3.8kg / min, the molten drop is 4-81 / s, the melting speed fluctuation range is ≤10%, and the molten drop range of the molten drop control statistics is 3-101 / s. The vacuum degree is ≤0.5Pa, and the leakage rate is ≤0.5.