Sintering process of ultra-fine grain WC hard alloy

By setting the appropriate hydrogen insulation section and hydrogen flow after hydrogen dewaxing, the problem of uncontrollable carbon content caused by fluctuations in oxygen content during sintering of ultrafine crystal WC cemented carbide is solved, and the stability and performance of the alloy carbon content are achieved promote.

CN119040683APending Publication Date: 2024-11-29ZIGONG CEMENTED CARBIDE CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159446.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Ultrafine crystal WC cemented carbide is uncontrollable due to fluctuations in oxygen content during sintering, which is prone to decarbonization or carburization, affecting the alloy performance.

Method used

After hydrogen dewaxing, set a hydrogen insulation section of 470℃ to 500℃ and a hydrogen flow rate of 10~15L/min to achieve the reduction of cobalt oxide and tungsten oxide by hydrogen, reduce the reaction between oxide and carbon at high temperature, and ensure the carbon content of the alloy In the expected range.

Benefits of technology

It effectively avoids deoxygenation and decarbonization of the alloy during vacuum solid phase sintering, reduces the reaction of hydrogen and tungsten carbide, ensures the stability of the alloy carbon content, and improves the performance of cemented carbide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006016150000051
    Figure BDA0005006016150000051
  • Figure BDA0005006016150000052
    Figure BDA0005006016150000052
  • Figure BDA0005006016150000061
    Figure BDA0005006016150000061
Patent Text Reader

Abstract

The invention belongs to the technical field of hard alloy sintering, and discloses a sintering process of an ultra-fine grain WC hard alloy, which comprises the following steps: after hydrogen dewaxing is completed, setting a proper hydrogen feeding heat preservation section and a proper hydrogen flow so as to realize reduction of most of oxides such as cobalt oxide and tungsten oxide in a pressed blank by hydrogen; the carbon loss in the alloy caused by the reaction of excessive oxides in the pressed blank with carbon at a higher temperature is reduced, the decarburization of the product caused by the reaction of hydrogen and tungsten carbide at a higher temperature and a large hydrogen flow can be avoided, and the carbon content of the alloy is ensured to be within an expected target range. The process can effectively solve the problem that the carbon content of the alloy is uncontrollable due to fluctuation of the oxygen content in the production process of the ultra-fine grain WC hard alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cemented carbide sintering, and more specifically relates to a sintering process of ultrafine-grained WC cemented carbide. Background Art

[0002] Ultrafine grain (WC grain size ≤ 0.6μm) WC cemented carbide is widely used in the field of cutting tools and wear-resistant parts due to its excellent hardness and wear resistance, good fracture strength and toughness. Ultrafine grain WC cemented carbide is made of sub-fine and below WC powder (Fsss grain size <1.0μm), fine grain (Fsss grain size 1.0~1.3μm) cobalt powder / nickel powder and transition metal carbide inhibitor (VC, Cr3C2, Mo2C, NbC, TaC, TiC and ZrC, etc.) and molding agent (paraffin, PEG, etc.), through wet grinding, vacuum drying, pressing and sintering.

[0003] The sintering process of cemented carbide can be divided into three types according to the dewaxing method: vacuum dewaxing vacuum sintering, hydrogen micro-positive pressure dewaxing vacuum / low-pressure sintering and argon pressure difference (negative pressure) dewaxing low-pressure sintering. At present, most domestic cemented carbide manufacturers mainly use hydrogen micro-positive pressure dewaxing vacuum / low-pressure sintering and argon pressure difference (negative pressure) dewaxing low-pressure sintering. In the production process of cemented carbide, the control of carbon content is the core of cemented carbide quality control. Due to the long production process of cemented carbide and many factors affecting the carbon-oxygen balance in the production process, it is very complicated and difficult to accurately control the carbon content in the production process. Compared with cemented carbides of other grain sizes, ultrafine grain WC cemented carbide is more easily affected by equipment and process factors in actual production. Ultrafine WC powder is prone to agglomeration and oxidation due to its large specific surface area and high surface activity, and the prepared mixture has a high oxygen content. In addition, as the mixture or green compact is placed for a longer time, the oxygen content of the mixture and green compact will further increase. Therefore, it is difficult to control the carbon-oxygen balance of such mixture and green compact during the sintering stage. It is easy to cause the alloy carbon content to be low (i.e., low cobalt magnetism) or even the presence of decarburized phase due to deoxidation and decarburization during the vacuum solid phase sintering stage. When the carbon content of the mixture is too high, carburization will occur in the alloy. The decarburized phase and carburized phase in the cemented carbide will greatly reduce the performance of the alloy.

[0004] Therefore, how to provide a sintering process for ultrafine-grained WC cemented carbide is a problem that those skilled in the art need to solve urgently. Summary of the invention

[0005] In order to overcome the shortcomings and deficiencies in the prior art, the present invention provides a sintering process for ultrafine-grained WC cemented carbide. After hydrogen dewaxing is completed (in order to avoid paraffin cracking and carburization of the alloy, the dewaxing temperature is set to ≤420°C), a suitable hydrogen insulation section (470°C to 500°C) and a suitable hydrogen flow rate (10 to 15L / min) are set to achieve hydrogen reduction of most oxides such as cobalt oxide and tungsten oxide in the compact, reducing the excessive oxides in the compact reacting with carbon at a higher temperature (700°C to 1000°C) and causing carbon loss in the alloy, and avoiding the reaction of hydrogen with tungsten carbide at a higher temperature and a large hydrogen flow rate to decarburize the product, ensuring that the carbon content of the alloy is within the expected target range. This process can effectively solve the problem of uncontrollable carbon content in the alloy due to fluctuations in oxygen content during the production of ultrafine-grained WC cemented carbide.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A sintering process for ultrafine-grained WC cemented carbide comprises the following steps:

[0008] (1) Hydrogen dewaxing stage: the ultrafine WC mixture compact is placed in a hydrogen dewaxing low-pressure sintering furnace, the hydrogen flow rate is controlled to be 10-25 L / min, the temperature is raised from room temperature to 280°C and kept at a certain heating rate, then raised to 380°C and kept at a certain temperature, and then slowly raised to 420°C and kept at a certain temperature, to complete the dewaxing;

[0009] (2) Hydrogen reduction oxide stage: Control the hydrogen flow rate, raise the temperature from 420°C to 470°C~500°C, and then keep warm;

[0010] (3) Vacuum sintering stage: After the insulation is completed, vacuum sintering is carried out, the temperature is raised to 1230°C and maintained, and then the temperature is raised from 1230°C to 1350°C and maintained. After the insulation is completed, argon gas is introduced to adjust the vacuum degree in the furnace to 3.0-5.0 KPa, and the temperature is raised from 1350°C to 1400°C-1440°C;

[0011] (4) Pressure sintering stage: When the temperature rises to 1400℃~1440℃, close the vacuum valve, introduce argon into the furnace, and keep the temperature and pressure at 1400℃~1440℃ for 60~90min; then cool to room temperature with the furnace to complete the sintering.

[0012] Preferably, in step (1), the temperature is raised from room temperature to 280°C at a rate of 3-4°C / min, and the holding time is 30 min.

[0013] Preferably, in step (1), the temperature is raised to 380° C. at a rate of 1 to 1.5° C. / min, and the holding time is 30 to 180 min.

[0014] Preferably, in step (1), the temperature is raised to 420° C. at a rate of 0.8 to 1.2° C. / min, and the holding time is 30 to 60 min.

[0015] Preferably, in step (2), the hydrogen flow rate is controlled to be 10 to 15 L / min.

[0016] Preferably, the insulation time in step (2) is 30 to 60 minutes.

[0017] The beneficial effects of the above technical solution are as follows: the WC powder and cobalt powder used in ultrafine and below grain cemented carbide are relatively fine in particle size and have a relatively high oxygen content. In addition, the ball milling time required to prepare such alloys is relatively long, and the oxygen content increases more after ball milling. The oxygen content of the prepared mixture and compact will further increase with the extension of storage time, and finally the oxygen content of such mixture and compact is 1.5 to 2 times that of the medium and coarse grain mixture and compact. If the oxygen content in the compact is too high, the excessive oxygen will react with the free carbon in the compact and the carbon in tungsten carbide in the range of 700 to 1000°C, resulting in excessive carbon loss in the alloy (MeO+C→Me+CO↑).

[0018] After hydrogen dewaxing is completed, the present invention sets appropriate temperature, hydrogen flow rate and holding time to achieve the purpose of reducing most of the oxygen in the compact by hydrogen (MeO+H2→Me+H2O↑, the amount of oxides reduced by hydrogen is related to temperature and time, and the amount of oxides reduced is ≥85% when the temperature is kept at 470-500°C for 1 hour). This not only avoids deoxidation and decarburization of the alloy during vacuum solid phase sintering, but also avoids the reaction of hydrogen with tungsten carbide at a relatively high temperature and a large hydrogen flow rate to decarburize the product (WC+2H2→CH4↑+W, the reaction is accelerated as the temperature increases and the hydrogen flow rate increases), thereby ensuring that the carbon content of the alloy is within the expected target range.

[0019] Preferably, in step (3), the temperature is raised to 1230° C. at a rate of 4 to 5° C. / min, and the holding time is 30 to 60 min.

[0020] Preferably, in step (3), the temperature is raised from 1230°C to 1350°C at a rate of 2.5-3.5°C / min, and the holding time is 30 min.

[0021] Preferably, in step (3), the temperature is increased from 1350°C to 1400°C to 1440°C at a rate of 4 to 5°C / min.

[0022] Preferably, in step (4), argon is introduced to make the pressure in the furnace reach 0.9-5.0 MPa, and the argon filling time is 6-30 minutes.

[0023] It can be seen from the above technical solution that, compared with the prior art, the present invention provides a sintering process for ultrafine-grained WC cemented carbide, which has the following advantages:

[0024] (1) The present invention optimizes the design of the hydrogen micro-positive pressure dewaxing process and sets a hydrogen insulation section at 470°C to 500°C after the hydrogen dewaxing is completed. This can not only more effectively reduce the oxides in the pressed green body and reduce the carbon loss caused by deoxidation and decarburization in the solid phase process, but also avoid the decarburization of the product caused by the reaction of hydrogen and tungsten carbide at a higher temperature, thereby greatly reducing the problem of uncontrollable carbon content in the alloy due to fluctuations in oxygen content during the production of ultrafine-grained WC cemented carbide.

[0025] (2) Under the premise of ensuring the efficiency of hydrogen micro-positive pressure dewaxing and the efficiency of hydrogen reducing oxides, the present invention can appropriately reduce the hydrogen flow rate when the room temperature rises to 280°C (before the paraffin evaporates rapidly) and from 420°C to 470-500°C (hydrogen reducing oxides), which can save hydrogen consumption to a certain extent and reduce production costs. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The present invention uses a compact prepared from a WC-3.5wt%Co-x wt%Cr ultrafine paraffin mixture as an experimental object, and conducts a sintering experiment in a hydrogen dewaxing low-pressure sintering experimental furnace. Before pressing the sample, the oxygen content of the batch of mixture is measured to be 0.57wt% (the oxygen content of a normal ultrafine mixture is generally 0.42wt% to 0.46wt%), and the pressed sample is vacuum-packed in a plastic bag and stored in a drying dish for use.

[0028] Example 1

[0029] A sintering process for ultrafine-grained WC cemented carbide comprises the following steps:

[0030]

[0031] Example 2

[0032] A sintering process for ultrafine-grained WC cemented carbide comprises the following steps:

[0033]

[0034]

[0035] Comparative Example 1

[0036] The sintering process of traditional ultrafine-grained WC cemented carbide includes the following steps:

[0037]

[0038] Comparative Example 2

[0039] The sintering process of traditional ultrafine-grained WC cemented carbide includes the following steps:

[0040]

[0041] Comparative Example 3

[0042] The sintering process of traditional ultrafine-grained WC cemented carbide includes the following steps:

[0043]

[0044]

[0045] The physical properties of the alloy samples of various embodiments and comparative examples are shown in Table 1:

[0046] Table 1

[0047]

[0048] As shown in Table 1, the cobalt magnetism of the cemented carbide samples obtained in Examples 1-2 of the present invention is qualified and within the internal control standard range, while in the traditional hydrogen dewaxing sintering process used in Comparative Examples 1-3, whether the hydrogen holding time in the dewaxing stage is extended or the hydrogen flow rate is increased, the cobalt magnetism of the cemented carbide samples obtained is low and unqualified. Therefore, the ultrafine-grained WC cemented carbide sintering process provided by the present invention can effectively control the carbon-oxygen balance during the alloy sintering process, reduce the difficulty of carbon content control, and ensure that the alloy cobalt magnetism meets the internal control standard.

[0049] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the scheme disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0050] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A sintering process for ultrafine-grained WC cemented carbide, characterized in that: The following steps are involved: (1) Hydrogen dewaxing stage: the ultrafine WC mixture compact is placed in a hydrogen dewaxing low-pressure sintering furnace, the hydrogen flow rate is controlled to be 10-25 L / min, the temperature is increased from room temperature to 280°C and kept at a certain heating rate, then increased to 380°C and kept at a certain temperature, and then slowly increased to 420°C and kept at a certain temperature, and the dewaxing is completed; (2) Hydrogen reduction oxide stage: Control the hydrogen flow rate, raise the temperature from 420°C to 470°C~500°C, and then keep warm; (3) Vacuum sintering stage: After the insulation is completed, vacuum sintering is carried out, the temperature is raised to 1230°C and maintained, and then the temperature is raised from 1230°C to 1350°C and maintained. After the insulation is completed, argon gas is introduced to adjust the vacuum degree in the furnace to 3.0-5.0 KPa, and the temperature is raised from 1350°C to 1400°C-1440°C; (4) Pressure sintering stage: When the temperature rises to 1400℃~1440℃, close the vacuum valve, introduce argon into the furnace, and keep the temperature and pressure at 1400℃~1440℃ for 60~90min; then cool to room temperature with the furnace to complete the sintering.

2. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: In step (1), the temperature is raised from room temperature to 280°C at a rate of 3-4°C / min, and the holding time is 30 min.

3. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: In step (1), the temperature is raised to 380° C. at a rate of 1 to 1.5° C. / min, and the heat preservation time is 30 to 180 min.

4. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: In step (1), the temperature is raised to 420° C. at a rate of 0.8 to 1.2° C. / min, and the heat preservation time is 30 to 60 minutes.

5. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: In step (2), the hydrogen flow rate is controlled to be 10-15 L / min.

6. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: The insulation time in step (2) is 30 to 60 minutes.

7. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: In step (3), the temperature is raised to 1230° C. at a rate of 4 to 5° C. / min, and the holding time is 30 to 60 min.

8. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: In step (3), the temperature is raised from 1230°C to 1350°C at a rate of 2.5-3.5°C / min, and the holding time is 30 minutes.

9. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: In step (3), the temperature is raised from 1350°C to 1400°C to 1440°C at a rate of 4 to 5°C / min.

10. The sintering process of ultrafine-grained WC cemented carbide according to claim 1, characterized in that: In step (4), argon gas is introduced to make the pressure in the furnace reach 0.9-5.0 MPa, and the argon filling time is 6-30 minutes.