Copper alloy and preparation method and application thereof
During the preparation of copper alloy, Cr powder, Mo powder and Cu powder are mechanically alloyed in a flowing CO atmosphere, and activated carbon powder is added for vacuum annealing, which solves the problem of improving the strength and conductivity of copper alloy and achieves high strength and high conductivity copper alloys, suitable for energy-containing rod housing materials.
Patent Information
- Application Number
- CN202411461767.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-29
AI Technical Summary
On the premise of retaining the conductivity of copper as much as possible, how to greatly improve the strength of copper alloy and avoid oxidation of metal powder to ensure block performance.
By placing Cr powder, Mo powder and Cu powder in a flowing CO atmosphere environment for mechanical alloying, and adding a small amount of activated carbon powder before annealing, vacuum annealing and hot pressing sintering, the amount of activated carbon powder is controlled to be 0.1 to 0.5 wt.% is used to purify the metal powder, to produce carbide Cr23C6, and to improve the performance of the copper alloy.
Achieve high tensile strength (not less than 1000MPa) and high conductivity (not less than 46%) of copper alloys, while avoiding the formation of oxides, improving the overall performance of blocks, and suitable for energy-containing rod shells body material.
Smart Images

Figure CN119040688A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloys and discloses a copper alloy and a preparation method and application thereof. Background Art
[0002] Cu-Cr alloys are the mainstream alloy system in the current research and application of high-strength and high-conductivity copper alloys. The solid solubility of Cr element in copper at room temperature is less than 0.03wt.%, and it is almost impossible to dissolve in solid. Even at the eutectic point of 1076℃, the solubility is only 0.73wt.%. After aging precipitation, the dispersion strengthening effect is strong. Copper alloys are divided into three types of materials: high strength and high conductivity, high strength and medium conductivity, and medium strength and medium conductivity. Among them, high-strength and high-conductivity copper materials, as a structural functional material, have excellent comprehensive physical and mechanical properties, such as high tensile strength and high conductivity, and have good comprehensive industrial performance. They are widely used in many fields of modern industry.
[0003] Adding a third alloying element to a Cu-Cr alloy is a method to further improve the comprehensive properties of the alloy, but the selection of the third alloying element is very difficult. For example, the solubility of the Fe element at the eutectic temperature is 4wt.%, while it drops to 0.3wt.% at room temperature to form a copper-based solid solution and α-Fe. Although the Fe element has a high shear modulus, is cheap and easy to obtain, Fe diffuses slowly in Cu, and forms a supersaturated solid solution after solidification, and the solid solution of the Fe element is extremely harmful to the conductivity of the copper alloy. Therefore, heat treatment is usually used to promote the precipitation of Fe at low temperatures and restore the electrical conductivity of the alloy to achieve the purpose of regulating the strength and conductivity of the Cu-Fe alloy. The commercially available Cu-Fe-Ag-P copper alloy mainly forms a Fe2P strengthening phase by adding P elements and Fe elements, and improves its comprehensive properties by adding Ag elements to accelerate the precipitation of Fe2P, but can only produce high-strength medium-conductivity copper alloys, which limits its potential applications.
[0004] The presence of O element in copper alloy will bring about oxidation problems, reacting with the copper matrix to form oxides such as CuO and Cu2O, or reacting with alloying elements to produce oxides, which will weaken the mechanical effect and reduce the conductivity of the alloy. The degree of oxidation is closely related to the preparation process of the alloy. For example, copper alloys prepared by mechanical alloying or magnetron sputtering technology have a smaller oxidation weight gain than traditional powder metallurgy methods due to their fine structure. For Cu-Cr copper alloys, Cr powder is easily oxidized, resulting in poor conductivity of the alloy. Therefore, in the face of practical application needs, how to significantly improve the strength of copper alloys while sacrificing the conductivity of copper as little as possible still needs further exploration. Summary of the invention
[0005] The technical problem to be solved by the present invention is: how to significantly improve the strength of copper alloy during preparation while retaining the conductivity of copper as much as possible; at the same time, how to avoid oxidation of metal powder during preparation of copper alloy to ensure the performance of bulk material after annealing and sintering.
[0006] In order to solve the above technical problems, the present invention provides a copper alloy and a preparation method and application thereof.
[0007] On the one hand, the present invention provides a method for preparing a copper alloy, which comprises: placing Cr powder, Mo powder and Cu powder in a flowing CO atmosphere environment respectively, obtaining Cr-Mo-Cu alloy powder by mechanical alloying, and performing annealing treatment, and hot pressing and sintering to obtain the copper alloy;
[0008] The added amount of the activated carbon powder is 0.1 to 0.5 wt. % based on the mass of the Cr-Mo-Cu alloy powder.
[0009] Furthermore, in the method for preparing the copper alloy of the present invention, the Cr powder, Mo powder and Cu powder are kept at 200-300° C. for 1-2 hours in a flowing CO atmosphere.
[0010] Furthermore, in the method for preparing the copper alloy of the present invention, the flow rate of CO is 15 mL / min to 40 mL / min.
[0011] Furthermore, in the preparation method of the copper alloy of the present invention, the mechanical alloying includes: mechanically alloying Cr powder and Mo powder to obtain Cr-Mo alloy powder, and then performing secondary mechanical alloying on the Cr-Mo alloy powder and Cu powder to obtain Cu-Cr-Mo alloy powder.
[0012] Furthermore, in the method for preparing the copper alloy of the present invention, the copper alloy is composed of 4.3-5.0% Cr, 4.0-5.2% Mo, and the remainder Cu, in terms of mass percentage.
[0013] On the other hand, the present invention claims protection for a copper alloy prepared by the preparation method of the present invention.
[0014] Furthermore, in the copper alloy provided by the present invention, the tensile strength of the copper alloy is not less than 1000 MPa, the elongation after fracture is not higher than 10%, and the IACS is not less than 46%.
[0015] On the other hand, the present invention relates to the use of the above copper alloy in the preparation of energetic rod shell materials.
[0016] Furthermore, in the application provided by the present invention, the energetic rod shell material is used for formation fissure expansion.
[0017] The energetic rod shell material of the present invention is a shell of energetic material. Energetic material is a compound or mixture containing explosive groups or oxidants and combustibles, which can independently undergo chemical reactions and output energy. It is an important component of explosives, propellants, propellants and pyrotechnics. The energetic rod shell material of the present invention is a thermal decomposition type, which can be rapidly decomposed after being stimulated by a certain amount of energy and release a large amount of heat energy. This material is usually used in the production of explosives and pyrotechnics because they can quickly generate high temperature and high pressure, thereby causing explosions.
[0018] Compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects or advantages:
[0019] (1) The present invention places Cr powder, Mo powder and Cu powder in a flowing CO atmosphere environment, and adds a small amount of activated carbon powder before annealing. During vacuum annealing, the activated carbon powder can react with the oxygen adsorbed during mechanical alloying to generate carbon dioxide, which is then extracted by a high vacuum exhaust station. At the same time, the activated carbon powder can also reduce oxides to achieve the purpose of purifying metal powders. In addition, Cr powder and activated carbon powder react to generate carbide Cr 23 C6, carbide Cr 23 C6 helps to improve the performance of copper alloy. In order to avoid poor performance of copper alloy caused by residual activated carbon powder, the present invention has confirmed through performance tests that the amount of activated carbon powder added must be controlled below 0.5wt.%.
[0020] (2) The present invention adds refractory metal Mo as a third alloying element to the Cu-Cr alloy to improve the performance of the copper alloy. Refractory metal Mo has excellent high-temperature performance, high thermal conductivity, good electrical conductivity, and low expansion coefficient, and can improve the heat resistance of the copper alloy. Mo and Cr both have a body-centered cubic BCC structure, which inhibits aging precipitation and prevents the abnormal growth of the precipitated phase due to excessive precipitation speed. In addition, Mo can also be used as a strengthening phase for dispersion-strengthened copper-based composite materials. Its solid solubility is extremely low and does not produce lattice distortion, and its electrical conductivity is much higher than that of compound particles. Therefore, while dispersion strengthening and increasing the softening temperature, it avoids a significant impact on the electrical conductivity of copper. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the description are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1The metallographic diagram of the copper alloy is shown in Figure 1. Among them, a is the copper alloy without adding activated carbon powder; b is the copper alloy provided in Example 3; and c is the copper alloy with adding 1.0wt.% activated carbon powder.
[0023] Figure 2 1500× metallographic diagram of the copper alloy. Among them, a is the copper alloy of Example 1; b is the copper alloy of Comparative Group 2.
[0024] Figure 3 This is the energetic rod assembled in Example 7. DETAILED DESCRIPTION
[0025] The technical scheme of the present invention is described below in conjunction with the embodiments, but the present invention is not limited to the following embodiments. The experimental methods and detection methods described in each embodiment are conventional methods unless otherwise specified; the reagents and materials described are all commercially available unless otherwise specified.
[0026] The invention provides a specific preparation process of the copper alloy.
[0027] Raw materials: Cu powder (purity 99.8%, particle size 200 mesh, Chengdu Huarui Metal Materials Co., Ltd.), Mo powder (99.5%, 200 mesh, Chengdu Huarui Metal Materials Co., Ltd.), Cr powder (99.5%, 200 mesh, Chengdu Huarui Metal Materials Co., Ltd.), activated carbon powder (99.8%, Tianjin Tianli Chemical Reagent Co., Ltd.).
[0028] Preparation process:
[0029] Step 1: Place Cr powder, Mo powder and Cu powder in a flowing CO atmosphere environment, keep them at 200-300°C for 1-2 hours, and the flow rate of CO is 15 mL / min-40 mL / min.
[0030] Step 2: Use a medium-sized high-energy horizontal vibrating rod mill (vibrating horizontal, the inner height of the tank is 550mm, and the inner diameter is 95mm) to mechanically alloy Cr powder and Mo powder for 4 hours to obtain Cr-Mo alloy powder, and then perform secondary mechanical alloying on the Cr-Mo alloy powder and Cu powder to obtain Cu-Cr-Mo alloy powder. Before rod milling, clean the inner wall of the rod mill tank and the stainless steel rod and dry them to avoid contamination of the powder. After the powder is filled and sealed, use a vacuum pump to evacuate the vacuum, and then fill with argon as an atmosphere protection. This process is repeated 2 to 3 times to prevent the powder from oxidizing during the rod milling process. For the rod milling of Cu-Cr-Mo alloy powder, an appropriate amount of n-heptane needs to be added as a process control agent to prevent cold welding. During the rod milling process, cooling water needs to be passed to reduce the cold welding of the powder and promote the formation of metastable state. After the rod milling is completed, stop the machine, and use anhydrous ethanol for protection to prevent oxidation or spontaneous combustion of the powder. After the wet powder is left to settle, the upper clear liquid is filtered out, placed in a vacuum drying oven, dried at 75°C for 6 hours, and sealed for storage.
[0031] Step 3: Mix the Cu-Cr-Mo alloy powder obtained in step 2 with activated carbon powder, the amount of activated carbon powder used is 0.1-0.5wt.% of the Cr-Mo-Cu alloy powder, mix well, put into a porcelain boat, and then put it into a tubular sintering furnace, and use a molecular pump to evacuate the tube to 10 -2 Pa and keep it, annealing at 600 ° C for 1 h, and finally cooling with the furnace to obtain the powder to be sintered.
[0032] Step 4: Fill the powder to be sintered obtained in step 3 into the cavity of a high-temperature alloy mold, and affix high-purity graphite paper to the inner wall of the cavity in contact with the powder. Use a pressure testing machine to pressurize to 630 MPa, maintain the pressure for 15 minutes, and then reduce the pressure to the pressure required for hot pressing sintering (500 MPa). The sintering furnace is heated at a heating rate of 10°C / min, and after reaching 900°C, it is kept warm for 2 hours, and finally cooled by 5°C / min. After cooling to normal room temperature, the pressure is released, and samples are taken to obtain a copper alloy.
[0033] Example 1
[0034] This embodiment provides a copper alloy and a preparation process thereof.
[0035] The preparation process refers to the specific preparation process of the above-mentioned copper alloy, except that the Cr powder, Mo powder and Cu powder are respectively placed in a flowing CO atmosphere environment and kept at 200°C for 1h; the flow rate of CO is 15mL / min; based on the mass of the Cr-Mo-Cu alloy powder, 0.1wt.% of activated carbon powder is added before the annealing treatment; in terms of mass percentage, the copper alloy is composed of 4.3% Cr, 4.0% Mo, and the remainder is Cu and unavoidable impurities.
[0036] Example 2
[0037] This embodiment provides a copper alloy and a preparation process thereof.
[0038] The preparation process refers to the specific preparation process of the above-mentioned copper alloy, except that the Cr powder, Mo powder and Cu powder are respectively placed in a flowing CO atmosphere environment and kept at 250°C for 1.5h; the flow rate of CO is 25mL / min; based on the mass of the Cr-Mo-Cu alloy powder, 0.3wt.% of activated carbon powder is added before the annealing treatment; in terms of mass percentage, the copper alloy is composed of 4.9% Cr, 5.1% Mo, and the remainder is Cu and unavoidable impurities.
[0039] Example 3
[0040] This embodiment provides a copper alloy and a preparation process thereof.
[0041] The preparation process refers to the specific preparation process of the above-mentioned copper alloy, except that the Cr powder, Mo powder and Cu powder are respectively placed in a flowing CO atmosphere environment and kept at 300°C for 2h; the flow rate of CO is 40mL / min; based on the mass of the Cr-Mo-Cu alloy powder, 0.5wt.% of activated carbon powder is added before the annealing treatment; in terms of mass percentage, the copper alloy is composed of 5.0% Cr, 5.2% Mo, and the remainder is Cu and unavoidable impurities.
[0042] Example 4
[0043] This example is intended to illustrate the effect of the amount of activated carbon powder added on the composition of the Cr-Mo-Cu alloy powder and the properties of the copper alloy.
[0044] The preparation method of the comparative sample is the same as that of Example 3, except that, based on the mass of the Cr-Mo-Cu alloy powder, 1.0 wt. % activated carbon powder is added before the annealing treatment, or no activated carbon powder is added.
[0045] The annealed Cr-Mo-Cu alloy powder was subjected to XRF testing. The test results are shown in Table 1 and the metallographic images are shown in Table 1. Figure 1 shown.
[0046] Table 1 XRF results of Cr-Mo-Cu alloy powder after annealing with different activated carbon powder contents
[0047] sample C (wt.%) O (wt.%) Fe(wt.%) No activated carbon powder added 0.00 3.36 0.94 Example 1 0.14 2.14 0.83 Example 2 0.39 1.82 0.84 Example 3 0.45 1.31 0.82 Add 1.0wt.% activated carbon powder 0.86 1.12 0.91
[0048] As shown in Table 1, the addition of activated carbon powder can significantly reduce the O content of the Cr-Mo-Cu alloy powder after annealing, and the content increases with the increase of the amount of activated carbon powder, and can also effectively reduce the Fe content. Figure 1As shown, when the amount of activated carbon powder is higher than 5.0wt.%, the matrix structure is the same, with gray reinforcement phase particles dispersed, but there are still residual carbon powder particles on the metallographic structure of the carbon annealed block. Comparing Example 3 with the sample with 1.0wt.% activated carbon powder added, it can be seen that the carbon powder particles in Example 3 are smaller, about 10μm or less, and the number is very small; the sample with 1.0wt.% activated carbon powder added has more residual carbon powder particles in the annealed block, the size of which can reach tens of microns, and the effect of reducing the Fe content is not obvious.
[0049] The electrical conductivity, tensile strength and elongation after fracture of the copper alloy block made from the annealed Cr-Mo-Cu alloy powder were measured. The measurement of electrical conductivity referred to GB / T 32791-2016 “Eddy current test method for electrical conductivity of copper and copper alloys”, and the measurement of tensile strength and elongation after fracture referred to GB / T228-2002 “Room temperature tensile test method for metallic materials”. The measurement results are shown in Table 2.
[0050] Table 2 Properties of copper alloy blocks after annealing with different activated carbon powder contents
[0051]
[0052] As shown in Table 2, the addition of activated carbon powder before annealing is beneficial to purify the formation of oxides in the copper alloy bulk material, improve the conductivity, tensile strength and elongation after fracture; in addition, when too much activated carbon powder is added, it will significantly reduce the performance of the copper alloy bulk material, which is not conducive to the use of the copper alloy bulk material for energetic rod shell materials. For energetic rod shell materials, the lower the elongation after fracture, the better, because it needs to be exploded into small fragments. Too high plasticity makes the shape of the material after explosion larger, which is not conducive to explosion.
[0053] Example 5
[0054] This example is intended to illustrate the effect of flowing CO atmosphere treatment on the properties of copper alloy.
[0055] During the two mechanical alloying processes, the powder is oxidized due to oxygen adsorbed on the powder surface and air not completely extracted from the rod mill. In particular, the Cr powder and Mo powder of the single mechanical alloying rod mill are prone to form chromium oxide and molybdenum oxide during the rod milling process. In addition, the insufficient vacuum degree of the vacuum drying box during the powder drying process will also cause a certain degree of powder oxidation. Therefore, a small amount of activated carbon powder is added during the annealing process. During vacuum annealing, it can react with the adsorbed oxygen to generate carbon dioxide and be extracted by the high vacuum exhaust table. At the same time, it can also reduce the oxide to achieve the purpose of purifying the powder. However, the addition of excessive activated carbon powder will lead to a decrease in the comprehensive performance of the copper alloy block, and the addition of too little activated carbon powder will have a small improvement effect on the copper alloy block. The purpose of the present invention to select a flowing CO atmosphere environment treatment is to be able to cooperate with the addition of activated carbon powder to synergistically achieve the improvement of the comprehensive performance of the copper alloy block, to achieve the purpose of improving the conductivity and tensile strength, and to have less effect on the elongation after fracture. A comparison group 1 is set, and the preparation method of the comparison group 1 is the same as that of Example 3, except that it is not placed in a flowing CO atmosphere environment. The electrical conductivity, tensile strength and elongation after fracture of the prepared copper alloy block were measured, and the test results are shown in Table 3.
[0056] Table 3 Effect of flowing CO atmosphere treatment on the properties of copper alloy bulk
[0057] sample Electrical conductivity (IACS,%) Tensile strength(MPa) Elongation after break (%) Example 1 47.43 1026.72 3.88 Example 2 48.64 1051.35 3.42 Example 3 47.98 1021.31 3.82 Comparison group 1 42.42 859.98 4.45
[0058] As shown in Table 3, the present invention selects the flowing CO atmosphere environment treatment, which can effectively cooperate with the activated carbon powder to improve the conductivity, tensile strength and elongation of the copper alloy block, which is close to the requirements of high-strength and high-conductivity copper. The present invention further tests the treatment effect of various gases, and the test results show that inert gas (such as Ar) or H2 has little effect on the conductivity, tensile strength and elongation of the copper alloy.
[0059] Example 6
[0060] This example is intended to illustrate the effect of the addition amounts of Mo and Cr on the properties of copper alloys.
[0061] A comparative group 2 was set up. The preparation method of the comparative group 2 was the same as that of Example 1, except that, in terms of mass percentage, the copper alloy consisted of 1.0% Cr, 1.0% Mo, and the remainder was Cu and unavoidable impurities. Multiple properties of the obtained copper alloy block were measured, and the test results are shown in Table 4.
[0062] Table 4 Effect of Mo and Cr addition on copper alloy properties
[0063] sample Example 1 Comparison group 2 Tensile strength(MPa) 1026.72 581.74 Elongation after break (%) 3.88 581.06 Yield strength (MPa) 836.31 516.06 Hardness (HV) 270.9 151.6 Relative density (%) 97.46 98.31 <![CDATA[Density (g / cm 3 )]]> 8.64 8.76
[0064] It can be seen from Table 4 that the copper alloy block with 4.3% Cr and 4.0% Mo content is the "critical point" of the comprehensive performance change trend. Since the solid solubility limit of Cr and Mo solid solution is relatively low during the secondary mechanical alloying process with Cu, for the copper alloy block provided by the composition of comparison group 1, the strengthening mode of the alloying elements is mainly dispersion strengthening rather than precipitation strengthening. The alloying elements with a content of 4.3% Cr and 4.0% Mo can improve the strength by pinning dislocations to achieve dispersion strengthening while avoiding the "splitting" effect on the copper matrix due to the excessive amount of second phase particles, resulting in a decrease in strength.
[0065] Figure 2 The high magnification (1500×) metallographic photographs of Example 1 and Comparative Group 2 are shown in FIG. Figure 2 It can be seen that after sintering, the copper grain size at the boundary of the powder particles is relatively large, and the grain boundary can be clearly observed. The size of the larger grain is about 1 to 2 μm. As the Cr and Mo contents increase, the coarse copper grain area at the powder boundary continues to decrease. The grains inside the powder particles are extremely fine, all below microns. As the content of alloying elements increases, the grains become finer, showing a more dense organization, and the size cannot be directly observed under an optical microscope. Except for a part of the strengthening phase particles being about 1 to 2 μm, most of them are below microns, and even cannot be observed at the nanoscale. However, as the Cr and Mo contents increase, the strengthening phase particles increase, and the size continues to increase, and even particles of 20 μm in size appear in composition embodiment 3. The grain size and strengthening phase particles play a decisive role in the comprehensive performance of copper alloys, especially ultrafine grained structures, and the comprehensive influence of grain boundaries on electrical conductivity and strength is more significant. With the increase of Cr and Mo content, on the one hand, the copper grains in the mechanical alloying powder are continuously refined, the fine grain strengthening is continuously enhanced, and the grain boundaries are also increased, which reduces the conductivity. On the other hand, the precipitation phase increases, and the solute atoms that are not precipitated in the copper matrix increase, which also affects the comprehensive performance.
[0066] Example 7
[0067] This example provides an experiment in which the copper alloy block prepared in Example 2 is used as an energetic rod shell material for formation fracture expansion.
[0068] Experimental process:
[0069] 1. Load the energetic material into the energetic rod shell (copper alloy block prepared in Example 2) to obtain multiple Figure 3 Energetic rod shown;
[0070] 2. Load 30 energetic rods into the shock wave generator;
[0071] 3. Send the shock wave generator to the operating depth of the oil well (4000m) through the oil pipe;
[0072] 4. Detonate the energetic rods on the ground through a remote control system;
[0073] 5. The shock wave generator automatically changes bullets;
[0074] 6. Repeat steps 4 and 5 until the job is complete.
[0075] Experimental results:
[0076] By generating shock waves at the same point multiple times to act on the formation, the energetic rod shell material can be broken into small pieces after blasting, promoting the development of formation fissures, generating micro-cracks, increasing the permeability of the rock formation near the wellbore, and thus improving the production efficiency of oil and gas wells. Experiments have shown that the radius of fracture development is greater than 16m.
[0077] The embodiments described above are part of the embodiments of the present invention, but not all of them. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. All other embodiments obtained without creative work and related deductions and substitutions made by ordinary technicians in the field under the conditions of the concept of the present invention belong to the scope of protection of the present invention.
Claims
1. A method for preparing a copper alloy, characterized in that: include: The Cr powder, Mo powder and Cu powder are placed in a flowing CO atmosphere environment respectively, and Cr-Mo-Cu alloy powder is obtained by mechanical alloying, and annealing is performed, and hot pressing and sintering is performed to obtain the copper alloy; The added amount of the activated carbon powder is 0.1 to 0.5 wt. % based on the mass of the Cr-Mo-Cu alloy powder.
2. The method for preparing the copper alloy according to claim 1, characterized in that: The Cr powder, Mo powder and Cu powder are kept at 200-300° C. for 1-2 hours in a flowing CO atmosphere.
3. The method for preparing the copper alloy according to claim 1, characterized in that: The flow rate of the CO is 15 mL / min to 40 mL / min.
4. The method for preparing the copper alloy according to claim 1, characterized in that: The mechanical alloying comprises: mechanically alloying Cr powder and Mo powder to obtain Cr-Mo alloy powder, and then performing secondary mechanical alloying on the Cr-Mo alloy powder and Cu powder to obtain Cu-Cr-Mo alloy powder.
5. The method for preparing the copper alloy according to claim 1, characterized in that: In terms of mass percentage, the copper alloy consists of 4.3-5.0% Cr, 4.0-5.2% Mo, and the balance Cu.
6. A copper alloy, characterized in that: The method is prepared by the method according to any one of claims 1 to 5.
7. The copper alloy according to claim 6, characterized in that The copper alloy has a tensile strength of not less than 1000 MPa, an elongation after fracture of not more than 10%, and an IACS of not less than 46%.
8. Use of the copper alloy described in claim 6 in the preparation of energetic rod shell materials.