Ultrafine grain seamless cupronickel thin-wall pipe and preparation method thereof

Through the process steps of vacuum casting, hot forging, mechanical processing, strong spinning and annealing heat treatment, ultra-fine grain white copper thin-walled pipes are formed, which solves the problems of easy corrosion and long process flow of white copper pipes in the existing technology, and significantly improves the The mechanical properties and corrosion resistance of the material are extended and the service life is extended.

CN119040689APending Publication Date: 2024-11-29YANTAI WANLONG VACUUM METALLURGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411156126.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing copper pipes are prone to corrosion in offshore equipment, and the existing preparation process is long and costly, so it is impossible to obtain fine grains of tissue, and the impact resistance and corrosion resistance of the material cannot be significantly improved.

Method used

Using a comprehensive process step of vacuum melt casting, hot forging, mechanical processing, strong spinning and annealing heat treatment, ultrafine grains are formed through high-purity melt, strict control of raw material ratio, large deformation processing and accumulated plastic deformation. Processing is performed to release residual stress and maintain the ultrafine crystal structure.

Benefits of technology

The ultrafine crystal seamless white copper thin-walled pipe with excellent mechanical properties and corrosion resistance was prepared, which significantly improved the application performance and service life of the material, avoided oxide generation and thermal stress defects, and realized large deformation calorimetric processing. Reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040689A_ABST
    Figure CN119040689A_ABST
Patent Text Reader

Abstract

The invention discloses an ultra-fine grain seamless cupronickel thin-wall pipe and a preparation method thereof, and the preparation method comprises the following steps: vacuum casting: under the condition that the vacuum degree is-0.1 MPa, melting and casting cupronickel alloy raw materials comprising the following components in percentage by weight: 10.0-11.0% of Ni, 1.0-1.8% of Fe, 0.5-1.0% of Mn and the balance of Cu into a cast ingot; hot forging cogging is conducted, specifically, hot forging treatment at 900-950 DEG C is conducted on the cast ingot, and the hot forging treatment comprises upsetting and drawing, punching and chambering till the size needed by the thin-wall pipe is achieved; machining is conducted, specifically, the hot-forged thin-wall pipe is machined so that the preset size precision can be achieved; powerful spinning: carrying out a plurality of times of powerful spinning on the thin-wall pipe so as to enable the accumulated thinning rate to reach a preset numerical value; annealing heat treatment is conducted, specifically, annealing heat treatment is conducted on the spun thin-wall pipe, the annealing temperature is controlled to be 680-740 DEG C, and the heat preservation time is 1-2 hours; and accurate grinding and polishing are conducted, specifically, the annealed thin-wall pipe is subjected to accurate grinding and polishing. According to the technical scheme, preparation of the ultra-fine grain seamless cupronickel thin-wall pipe is achieved through a series of accurately-controlled process steps.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tube preparation, and in particular relates to an ultrafine-grained seamless white copper thin-wall tube and a preparation method thereof. Background Art

[0002] At present, white copper alloy pipes have broad application prospects in fields such as marine engineering equipment. With the expansion of application fields, higher and higher requirements are placed on the comprehensive performance of white copper pipes, such as strength, elongation, and erosion and corrosion resistance.

[0003] In actual applications, the existing nickel silver tube products for offshore equipment are very susceptible to corrosion due to long-term impact from seawater. By improving the comprehensive properties such as strength and elongation, the impact resistance of the material can be significantly improved, thereby improving the erosion corrosion resistance of the pipe. Fine grain strengthening is a strengthening method that can simultaneously improve the strength and elongation of the material. Therefore, through a reasonable preparation method, the ultrafine grain microstructure can be obtained, which will significantly improve the erosion corrosion resistance of the nickel silver tube products for offshore equipment, thereby extending its service life.

[0004] At present, domestic large-diameter nickel silver tubes are mainly prepared by the "extrusion, expansion and pulling" process. This method not only requires large equipment investment and a long process flow, but also cannot strengthen the alloy material through grain refinement due to the small deformation. Later, someone proposed a method of preparing large-diameter nickel silver thin-walled tubes by the "ingot hot forging + composite extrusion + spinning" process. The specific process is: ingot → hot forging → hot extrusion → machining → spinning → heat treatment → finishing and polishing. This method has the following limitations:

[0005] 1) The process is long and requires multiple deformation processes such as hot forging and extrusion, resulting in high production costs;

[0006] 2) The weight and size of the produced tube are limited by the specifications of the extrusion die barrel, and hot processing with large deformation cannot be performed, so a fine-grained structure cannot be obtained. Summary of the invention

[0007] The object of the present invention is to provide an ultrafine-grained seamless white copper thin-wall tube and a preparation method thereof, thereby solving at least part of the above-mentioned technical problems.

[0008] A first aspect of an embodiment of the present invention provides a method for preparing an ultrafine-grained seamless white copper thin-wall tube, comprising the following steps:

[0009] Vacuum melting and casting: Under the condition of a vacuum degree of -0.1 MPa, a white copper alloy raw material containing Ni: 10.0-11.0%, Fe: 1.0-1.8%, Mn: 0.5-1.0%, and Cu as the balance in weight percentage is melted and cast into an ingot;

[0010] Hot forging: The ingot is hot forged at 900-950℃, including upsetting, punching and expanding, until the required size of the thin-walled tube is reached;

[0011] Machining: Machining the thin-walled tube after hot forging to achieve the predetermined dimensional accuracy;

[0012] Power spinning: several passes of power spinning are performed on thin-walled pipes to make the cumulative thinning rate reach a predetermined value;

[0013] Annealing heat treatment: Annealing heat treatment is performed on the thin-walled tube after spinning. The annealing temperature is controlled at 680℃ to 740℃ and the insulation time is 1 hour to 2 hours;

[0014] Fine grinding and polishing: Fine grinding and polishing of thin-walled tubes after annealing.

[0015] The technical effect achieved is as follows: the technical solution of the present invention realizes the preparation of ultrafine-grained seamless white copper thin-walled tubes through a series of precisely controlled process steps. First, the vacuum casting step is carried out under a high vacuum condition of -0.1MPa, which effectively eliminates gas and impurities and avoids the formation of oxides, thereby ensuring the purity of the alloy melt. This high-purity melt is the basis for the formation of ultrafine grains. Secondly, the strictly controlled raw material ratio, especially the addition of trace elements, provides a chemical basis for the formation of a uniform alloy structure, which is one of the key factors for obtaining ultrafine grains. The hot forging step promotes the crushing and recrystallization of grains through large deformation processing at high temperature, further refining the grains. The strong spinning step increases the deformation of the material through continuous deformation, and this accumulated plastic deformation is an effective means to achieve ultrafine grain size. Finally, the annealing heat treatment step helps to release the residual stress inside the material, promotes the growth of grains to a more uniform size, and maintains the ultrafine grain structure. Through the combined effect of this series of steps, the present invention successfully prepares seamless white copper thin-walled pipes with ultrafine grain size. These ultrafine grains give the pipes excellent mechanical properties and corrosion resistance, significantly improving the application performance and service life of the material.

[0016] Optionally, in the vacuum melting and casting step, the melting temperature of the ingot is controlled between 1300°C and 1360°C.

[0017] The technical effect achieved is: controlling the melting temperature between 1300℃ and 1360℃ to ensure that the alloy components are fully melted and evenly mixed, while avoiding overheating that causes serious burning of elements.

[0018] Optionally, in the vacuum melting and casting step, the ingot mold used for the ingot is baked at 350° C. to 400° C. before smelting and kept warm for at least 12 hours.

[0019] The technical effects achieved are: baking the ingot mold to remove moisture and grease, reducing gas inclusions during the melting and casting process, and improving the purity and structural uniformity of the ingot.

[0020] Optionally, in the vacuum melting step, electrolytic copper, electrolytic nickel and iron nails are put into a crucible and heated to melt.

[0021] The technical effect achieved is: electrolytic copper, electrolytic nickel and iron nails are put into a crucible and melted at the same time, ensuring that these main alloy elements are dispersed during the smelting process to form a uniform alloy melt.

[0022] Optionally, when the temperature of the molten copper reaches 1300° C., electrolytic manganese is added to the molten copper.

[0023] The technical effect achieved is: electrolytic manganese is added when the temperature of the molten copper reaches 1300°C. This temperature control helps to ensure that the manganese element can be fully melted without causing severe oxidation and burning due to long-term heating.

[0024] Optionally, in the vacuum melting and casting step, pouring is performed when the temperature of the molten copper reaches 1350±10°C.

[0025] The technical effect achieved is: pouring is carried out when the copper liquid temperature reaches 1350±10℃. This temperature range is conducive to obtaining good ingot structure and performance, while avoiding the influence of overcooling or overheating on material properties.

[0026] Optionally, in the vacuum melting and casting step, the riser of the ingot mold is covered with insulation cotton after pouring, and the ingot is lifted out of the casting chamber after 1 hour to complete the cooling and solidification of the ingot.

[0027] The technical effect achieved is: after pouring, the ingot mold is insulated to ensure uniform cooling and solidification of the ingot, and to reduce casting defects such as thermal stress and shrinkage cavities.

[0028] Optionally, in the hot forging step, the thin-walled tube is drawn at 900° C. to 950° C., and is returned to the furnace for heating and kept warm for not less than 1 hour between each drawing and forging.

[0029] The technical effect achieved is: by pulling at 900℃ to 950℃, a large deformation amount can be achieved, grain refinement can be promoted, and the strength and toughness of the material can be improved.

[0030] Optionally, in the high-pressure spinning step, the single-pass thinning rate is controlled to be between 20% and 30%, the cumulative thinning rate is ≥75%, and the feed ratio is controlled to be between 1.5 and 2.5 mm / r.

[0031] The technical effect achieved is: controlling the single-pass thinning rate and cumulative thinning rate, as well as the feed ratio during the high-power spinning process to achieve uniform thinning of the tube wall thickness. Combined with subsequent annealing heat treatment, it can achieve the purpose of grain refinement and improve the mechanical properties of the material.

[0032] A second aspect of an embodiment of the present invention provides an ultrafine-grained seamless white copper thin-walled tube, which is made by the above method.

[0033] The technical effect achieved is: the ultrafine-grained seamless white copper thin-walled pipe prepared by any of the methods in claims 1 to 9 has excellent mechanical properties and corrosion resistance, and is particularly suitable for fields such as marine engineering equipment that have extremely high requirements for material properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a hot forged metallographic image of an ultrafine-grained seamless white copper thin-wall tube in an embodiment of the present invention;

[0035] Figure 2 The metallographic structure of a thin-walled ultrafine-grained seamless white copper tube in a spinning state in an embodiment of the present invention;

[0036] Figure 3 This is the annealed metallographic phase of an ultrafine-grained seamless white copper thin-wall tube in an embodiment of the present invention;

[0037] Figure 4 The present invention is a schematic flow chart of a method for preparing an ultrafine-grained seamless white copper thin-wall tube in an embodiment of the present invention. DETAILED DESCRIPTION

[0038] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The modes described in the following exemplary embodiments do not represent all modes consistent with the present invention. Instead, they are merely examples of devices consistent with some aspects of the present invention as detailed in the appended claims.

[0039] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present specification and claims do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "one" do not indicate a quantitative limitation, but indicate that there is at least one. If only "one" is referred to, it will be separately stated. "Multiple" or "several" means two or more. Unless otherwise specified, words such as "front", "rear", "lower" and / or "upper" are only for the convenience of explanation and are not limited to one position or one spatial orientation. Words such as "include" or "comprise" mean that the elements or objects appearing in front of "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. "Connected" or "connected" and similar words are not limited to physical or mechanical connections, and may include electrical connections, whether direct or indirect. The singular forms "a", "said" and "the" used in the present specification and the appended claims are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0040] The present invention discloses a method for preparing an ultrafine-grained seamless white copper thin-wall tube. Figure 4 As shown, the specific steps include: vacuum melting and casting, hot forging, machining, high-power spinning, annealing heat treatment and fine grinding and polishing.

[0041] The vacuum casting steps specifically include:

[0042] 1) The ingot mold, ingot mold base, launder and stopper rod are baked in advance at a baking temperature of 350-400°C for 12 hours.

[0043] 2) Ingredients: Ingredients are prepared according to the weight percentage of Ni: 10.0-11.0%, Fe: 1.0-1.8%, Mn 0.5-1.0%, and the balance of Cu.

[0044] 3) Smelting: Put the raw materials into the smelting chamber, among which electrolytic copper, electrolytic nickel and iron nails are weighed and directly added to the crucible, and electrolytic manganese is placed in the small silo above. After the melting chamber is closed, vacuum is evacuated, and the vacuum degree reaches -0.1MPa, which is maintained until the ingot casting is completed, and power is supplied to increase the temperature. 30 minutes before the copper water is melted, the ingot mold assembly is started, and the assembled ingot mold and the tundish are hoisted into the casting chamber, and then vacuum is evacuated after closing. After the copper water is melted, the temperature is measured with a temperature measuring rod. When the temperature of the copper water reaches 1300℃, there is no need to break the vacuum. Open the partition below the small silo and put in electrolytic manganese; heat up to 1340-1360℃ with high power and keep the temperature constant for 5-10 minutes; let it stand until the temperature of the copper water is 1350±10℃ and then introduce it into the tundish; let it stand again, and when the temperature of the copper water drops to 1180-1200℃, move the plug rod to pour the copper alloy melt into the ingot mold. After breaking the vacuum, the tundish is lifted out and the riser of the ingot mold is covered with insulation cotton. After 1 hour, it is lifted out of the casting chamber and the ingot casting is completed.

[0045] The hot forging process specifically includes:

[0046] 1) Pulling and drawing: Three pulls and three draws are carried out at 900-950℃, and the deformation of each pull and drawing is ≥50%. The gap between each pull and drawing is returned to the furnace for heating and heat preservation for ≥1h;

[0047] 2) Punching and expanding: Punching at 900-950℃ and expanding to φ280mm. Ensure the terminal temperature is ≥850℃;

[0048] 3) Hot forging and drawing: 900-950℃ hot forging and drawing to 2000mm. Ensure the terminal temperature is ≥850℃.

[0049] The mechanical processing steps specifically include: the copper tube blank after hot forging is processed by lathe to a suitable size without defects. The inner diameter of the processed copper sleeve blank is φ306mm and the wall thickness is 42-50mm.

[0050] The high-power spinning step specifically includes: using a three-wheel high-power spinning machine to perform several passes of spinning, with a single pass thinning rate of 20-30%, a cumulative thinning rate of ≥75%, and a feed rate of 1.5-2.5mm / r. The spinning method is reverse spinning.

[0051] The annealing heat treatment step specifically includes: bright annealing furnace annealing, annealing temperature 680-740° C., and heat preservation time 1-2 hours.

[0052] The fine grinding and polishing steps specifically include: grinding with a special polishing machine, and the outer diameter tolerance of the pipe after fine grinding and polishing is ≤±0.5mm, the wall thickness tolerance is ≤±0.2mm, and the straightness is ≤3mm / m.

[0053] The process advantages include: first, the vacuum casting step is carried out under a high vacuum condition of -0.1MPa, which effectively eliminates gases and impurities and avoids the formation of oxides, thereby ensuring the purity of the alloy melt. This high-purity melt is the basis for the formation of ultrafine grains. Secondly, the strictly controlled raw material ratio, especially the addition of trace elements, provides a chemical basis for the formation of a uniform alloy structure, which is one of the key factors in obtaining ultrafine grains. The hot forging step promotes the crushing and recrystallization of grains through large deformation processing at high temperature, further refining the grains. The high-power spinning step increases the deformation of the material through continuous deformation, and this accumulated plastic deformation is an effective means to achieve ultrafine grain size. Finally, the annealing heat treatment step helps to release the residual stress inside the material and promote the growth of grains to a more uniform size while maintaining the ultrafine grain structure. Through the combined effect of this series of steps, the present invention successfully prepares seamless white copper thin-walled pipes with ultrafine grain size. These ultrafine grains give the pipes excellent mechanical properties and corrosion resistance, significantly improving the application performance and service life of the material.

[0054] At the same time, the above preparation method does not require hot extrusion, the weight is not limited to the specifications of the extrusion die barrel, and hot processing with large deformation can be performed to obtain ultrafine grain structure, which is beneficial to the improvement of the comprehensive performance of the copper tube.

[0055] The processing object is B10 white copper alloy large-diameter seamless thin-walled pipe, the finished product has an outer diameter of 340mm, a wall thickness of 16mm and a length of 4000-4500mm.

[0056] According to the composition of B10 white copper alloy, it is melted in a vacuum induction melting furnace at a melting temperature of 1350℃; the raw materials are put into the melting chamber, among which electrolytic copper, electrolytic nickel and iron nails are weighed and directly added to the crucible, and electrolytic manganese is placed in the small silo above. After the melting chamber is closed, the vacuum is evacuated to a vacuum degree of -0.1MPa, which is maintained until the ingot casting is completed, and power is supplied to increase the temperature at the same time. When the temperature of the molten copper reaches 1300℃, open the partition below the small silo and put in electrolytic manganese; heat up to 1350℃ at high power and keep the temperature constant for 5min; let it stand and introduce the tundish when the temperature of the molten copper is 1350±10℃; let it stand again and pour the copper alloy melt into the ingot mold when the temperature of the molten copper drops to 1180℃. After breaking the vacuum, the tundish is lifted out, and the riser of the ingot mold is covered with insulation cotton. After 1 hour, it is lifted out of the casting chamber to complete the ingot casting.

[0057] First, the copper ingot is heated to 950℃ in a heating furnace for three-stage roughing and three-stage drawing. The deformation of each roughing and drawing is ≥50%; after returning to the furnace and heating and heat preservation at 950℃, the hole is punched and expanded to φ280mm; after returning to the furnace and heat preservation at 920℃, the hot forging and drawing are lengthened to 2000mm. The lathe is processed to φ390 / φ306×1960mm, and the inner diameter tolerance is +0.25mm. Samples are taken to observe the grains of the hot forged copper tube, such as Figure 1 shown.

[0058] A total of 3 passes of spinning were performed using a three-wheel high-power spinning machine, with thinning rates of 21%, 24.8%, and 22.5% respectively. The feed ratio of the first pass was 1.75mm / r, and the feed ratio of the next two passes was 2mm / r. The size after spinning is: φ346 / φ306×4080mm. Figure 2 shown.

[0059] After cutting off the head and tail machining allowances of the spun copper sleeve, annealing was performed at 740℃*1h and air cooling. Samples were taken for microstructure analysis, and the average grain size was 9um. Figure 3 shown.

[0060] Fine grinding and polishing: Use a special polishing machine for grinding. After fine grinding and polishing, the outer diameter tolerance of the pipe is ≤±0.5mm, the wall thickness tolerance is ≤±0.2mm, and the straightness is ≤3mm / m.

[0061] The size of the copper sleeve after fine grinding and polishing is φ340 / 306*4050mm, its tensile strength is greater than 360MPa, and its elongation is greater than 25%.

[0062] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing an ultrafine-grained seamless white copper thin-walled tube. It is characterized in that The preparation method comprises the following steps: Vacuum melting and casting: Under the condition of a vacuum degree of -0.1 MPa, a white copper alloy raw material containing Ni: 10.0-11.0%, Fe: 1.0-1.8%, Mn: 0.5-1.0%, and Cu as the balance in weight percentage is melted and cast into an ingot; Hot forging: The ingot is hot forged at 900-950℃, including upsetting, punching and expanding, until the required size of the thin-walled tube is reached; Machining: Machining the thin-walled tube after hot forging to achieve the predetermined dimensional accuracy; Power spinning: Perform several passes of power spinning on thin-walled pipes to make the cumulative thinning rate reach the predetermined value; Annealing heat treatment: Annealing heat treatment is performed on the thin-walled tube after spinning. The annealing temperature is controlled at 680℃ to 740℃ and the insulation time is 1 hour to 2 hours; Fine grinding and polishing: Fine grinding and polishing of thin-walled tubes after annealing.

2. A method for preparing an ultrafine-grained seamless white copper thin-walled tube according to claim 1, It is characterized in that In the vacuum melting and casting step, the melting temperature of the ingot is controlled between 1300°C and 1360°C.

3. The method for preparing an ultrafine-grained seamless white copper thin-walled tube according to claim 1, It is characterized in that In the vacuum melting and casting step, the ingot mold used for ingot casting is baked at 350° C. to 400° C. before smelting and kept warm for at least 12 hours.

4. The method for preparing an ultrafine-grained seamless white copper thin-walled tube according to claim 1, It is characterized in that In the vacuum melting step, electrolytic copper, electrolytic nickel and iron nails are put into a crucible and heated to melt.

5. The method for preparing an ultrafine-grained seamless white copper thin-walled tube according to claim 4, It is characterized in that When the temperature of the molten copper reaches 1300°C, electrolytic manganese is added into the molten copper.

6. The method for preparing an ultrafine-grained seamless white copper thin-walled tube according to claim 4, It is characterized in that In the vacuum casting step, pouring is performed when the temperature of the molten copper reaches 1350±10°C.

7. The method for preparing an ultrafine-grained seamless white copper thin-walled tube according to claim 6, It is characterized in that In the vacuum casting step, after pouring, the riser of the ingot mold is covered with insulation cotton, and after 1 hour, the ingot is lifted out of the casting chamber to complete the cooling and solidification of the ingot.

8. The method for preparing an ultrafine-grained seamless white copper thin-wall tube according to claim 1, It is characterized in that In the hot forging step, the thin-walled pipe is drawn at 900° C. to 950° C., and is returned to the furnace for heating and kept warm for not less than 1 hour between each drawing and forging.

9. The method for preparing an ultrafine-grained seamless white copper thin-walled tube according to claim 1, It is characterized in that In the high-power spinning step, the single-pass thinning rate is controlled to be between 20% and 30%, the cumulative thinning rate is ≥75%, and the feed ratio is controlled to be between 1.5 and 2.5 mm / r.

10. An ultra-fine-grained seamless white copper thin-walled tube, It is characterized in that The ultrafine-grained seamless white copper thin-walled tube is made by the preparation method described in any one of claims 1-9.

Citation Information

Cited By

  • Fine-grain and homogenized cupronickel tube and preparation method thereof

    CN120734135A

  • Preparation method of large-diameter seamless thin-walled tubular part