1235D lithium battery aluminum foil and preparation method thereof
By adjusting the addition amount of aluminum-titanium boron wire and annealing process, the elongation of the aluminum foil of 1235D lithium battery is improved, and the problem of insufficient elongation in the existing technology is solved, and the high tensile strength and elongation of the aluminum foil of lithium battery is achieved, which significantly improves the Performance stability of lithium-ion batteries.
Patent Information
- Application Number
- CN202411006612.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-29
AI Technical Summary
The elongation rate of the existing 1235D lithium battery aluminum foil is difficult to reach more than 4.0%, which limits the performance of lithium batteries in specific application scenarios. The tensile strength is improved but the elongation rate is insufficient, which affects the battery performance and life.
By regulating the addition amount of aluminum-titanium boron wire and annealing process, the cast-rolling structure and recrystallization structure are refined, the performance of aluminum alloy is improved by using Cu and Mn elements, double filtration is carried out to improve the purity of aluminum liquid, and intermediate annealing is performed during the cold rolling process. , improve the tensile strength and elongation of aluminum foil.
The obtained lithium battery aluminum foil can reach more than 4.0% while the tensile strength exceeds 240MPa, which significantly improves the performance stability and yield of lithium-ion batteries.
Smart Images

Figure BDA0004963171140000081 
Figure BDA0004963171140000082
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium battery aluminum foil, and in particular to a 1235D lithium battery aluminum foil and a preparation method thereof. Background Art
[0002] Battery aluminum foil is a key basic material for the positive electrode of lithium batteries. In lithium-ion batteries, aluminum foil, as the positive electrode current collector material, not only acts as a carrier of the positive electrode active material, but also collects the current generated by the positive electrode active material of the battery and conducts it to the external circuit, thereby realizing the process of converting chemical energy into electrical energy. Based on the requirement to increase the energy density of power batteries, battery aluminum foil has increasingly stringent requirements on thickness, conductivity, surface tension, tensile strength, elongation and other indicators.
[0003] At present, the elongation level of 1235D battery aluminum foil produced by enterprises is about 3.0%-3.5%. With the rapid development of new energy technologies, lithium batteries, as important energy storage devices, have increasingly higher performance requirements. As one of the important components of lithium batteries, the tensile strength and elongation of aluminum foil directly affect the performance and life of the battery. At present, although the tensile strength of battery aluminum foil on the market has been improved, the elongation is often difficult to reach more than 4.0%, which limits the performance of lithium batteries in specific application scenarios. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a 1235D lithium battery aluminum foil and a preparation method thereof. The present invention improves the elongation of the 1235D lithium battery aluminum foil by adjusting the amount of aluminum-titanium-boron wire added to finely and evenly form the cast-rolled structure and adjusting the annealing process to finely and evenly form the recrystallized structure. The prepared aluminum foil for lithium batteries has an elongation of more than 4.0% while having a tensile strength of more than 240 MPa, which is 33% higher than the elongation of the battery aluminum foil produced by the original process, thereby significantly improving the performance stability of lithium-ion batteries.
[0005] The present invention is achieved through the following technical solutions: on the one hand, a 1235D lithium battery aluminum foil is provided, the chemical composition of the lithium battery aluminum foil, by mass percentage, includes Si≤0.06%, Fe: 0.35%-0.45%, Cu: 0.11%-0.18%, Mn: 0.02%-0.04%, Ti: 0.015%-0.030%, H≤0.12mL / 100gAl, other single impurity elements ≤0.03%, and the balance is Al.
[0006] Through the above technical scheme, the present invention adds Cu and Mn elements to the aluminum alloy. The Cu element can form an AlFeCu phase with Fe, which has a certain degree of crushing during the rolling process. It promotes nucleation and recrystallization through particles, and plays a role in refining grains in the intermediate recrystallization process. At the same time, the precipitation of the Cu element has a pinning effect on the movement of dislocations, and can also effectively prevent the growth of grains. In short, the presence of the Cu element effectively improves the performance indicators of the aluminum alloy. The presence of the Mn element can form a chemical phase with Fe, thereby reducing the harmful effects of the Fe element, and can simultaneously increase the recrystallization temperature of the aluminum alloy, which plays an effective role in improving the strength and plasticity of the aluminum alloy.
[0007] During casting and rolling, double filtration is performed by using a tubular filter box and a ceramic filter plate. Double filtration can improve the purity of the aluminum liquid and reduce the defect rate of pinholes, airways, slag inclusions, etc. in the cast and rolled plate.
[0008] During the cold rolling process, intermediate annealing is carried out when the plate thickness is 1.5-1.8mm, which promotes the recrystallization of the deformed grains, transforms the slender grains into equiaxed grains, eliminates the work hardening of the rolled aluminum plate, and increases the plasticity and toughness of the rolled plate, which is beneficial to the deformation of the aluminum plate and the subsequent rolling.
[0009] Before casting and rolling, Al-Ti-B wire is added to the flow trough to modify the aluminum alloy by Ti and B, which can effectively reduce the grain size of the aluminum alloy and obtain a cast-rolled plate with fine and uniform grains.
[0010] Furthermore, the mass percentage of Al is ≥99.35%.
[0011] A method for preparing the above-mentioned 1235D lithium battery aluminum foil is also provided, comprising the following steps:
[0012] Step 1) Ingredients: Ingredients are prepared according to the composition standard of 1235D lithium battery aluminum foil, and the aluminum ingot raw material used is an electrolytic aluminum ingot with a purity of not less than 99.7%;
[0013] Step 2) Melting: Place the raw materials obtained in step 1) in a smelting furnace for melting. After the raw materials are melted, the obtained aluminum alloy liquid is refined, and alloy materials that meet the composition requirements of 1235D lithium battery aluminum foil are added to obtain aluminum alloy liquid.
[0014] Step 3) insulation: the aluminum alloy liquid obtained in step 2) flows into an insulation furnace for whole furnace refining;
[0015] Step 4) Degassing: Degassing and refining are performed using a degassing box, and aluminum-titanium-boron wires are added in batches before and after degassing, so that the Ti content in the aluminum alloy liquid is 0.015%-0.030%, and the B content is 0.0015%-0.0030%, ensuring that a fine and uniform casting and rolling structure is obtained, providing high-quality billets for the cold rolling process;
[0016] Step 5) Filtration: Using a filter box and a ceramic filter sheet to perform double-stage filtration on the aluminum alloy liquid;
[0017] Step 6) Casting and rolling: injecting the aluminum alloy liquid obtained in step 5) into the casting and rolling unit through the launder and casting trough for continuous casting and rolling to obtain a cast plate;
[0018] Step 7) cold rolling: cold rolling the cast-rolled sheet obtained in step 6) to a thickness of 0.20-0.25 mm, and performing intermediate annealing when the thickness is 1.6-2.0 mm and then continuing cold rolling;
[0019] Step 8) foil rolling: the cold rolled sheet obtained in step 7) is subjected to rough rolling, intermediate rolling and finish rolling to obtain aluminum foil with a thickness of 0.010-0.015 mm;
[0020] Step 9) Rewind, trim, inspect and package.
[0021] Through the above technical scheme, on the basis of adding appropriate amount of Al-Ti-B wire to refine the cast-rolled structure, the elongation of 1235D lithium battery aluminum foil is improved by adjusting the amount of aluminum-titanium-boron wire added to finely and evenly cast the rolled structure and adjusting the annealing process to finely and evenly recrystallize the structure. The obtained aluminum foil for lithium batteries has a tensile strength of more than 240MPa and an elongation of more than 4.0%, which is 33% higher than the elongation of battery aluminum foil produced by the original process, significantly improving the performance stability of lithium-ion batteries.
[0022] Furthermore, in step 1), the cold-rolled secondary waste in step 7) is recycled as raw material; wherein, the amount of the recycled cold-rolled secondary waste added is not higher than 5% of the total weight of the smelted aluminum alloy, thereby ensuring the cleanliness of the aluminum alloy and improving the performance stability of the lithium battery aluminum foil.
[0023] Furthermore, in step 2), the refining temperature is 740-750°C.
[0024] Furthermore, in step 4), the titanium content of the aluminum titanium boron wire is 4.5%-5.5%, and the B content is 0.8%-1.2%.
[0025] Furthermore, in step 5), the double-stage filtration includes a primary ceramic filter plate and a secondary ceramic filter plate; the primary ceramic filter plate is 50 mesh, and the secondary ceramic filter plate is 60 mesh; and the filtration temperature is 710°C-730°C.
[0026] Furthermore, in step 6), the casting temperature during casting and rolling is 688-693° C.; the thickness of the cast and rolled plate is 6.5-8.0 mm.
[0027] Further, in step 7), the cold rolling is performed in 5 passes, and the distribution scheme of each pass is: (6.5-8.0) mm→(3.2-3.6) mm→(1.6-2.0) mm→(0.6-0.9) mm→(0.3-0.4) mm→(0.20-0.25) mm.
[0028] Through the above technical solution, intermediate annealing is performed at a thickness of 1.6-2.0mm to adjust the matching degree of tensile strength and elongation. The greater the annealing thickness, the higher the subsequent processing hardening degree and strength, and the smaller the expected elongation of the aluminum foil; the smaller the annealing thickness, the lower the subsequent processing hardening degree and strength, and the higher the expected elongation of the aluminum foil; annealing thickness that is too large or too small will significantly reduce the process window for obtaining a suitable matching relationship between tensile strength and elongation. There is an optimal annealing thickness to maximize the allowable fluctuation range of composition and process.
[0029] Furthermore, in step 7), the intermediate annealing conditions are: the annealing furnace gas temperature is 480-530°C, the holding time is 20-25 hours, and then air-cooled to room temperature. Under the above annealing thickness and annealing process conditions, a fine and uniform recrystallized structure can be obtained.
[0030] The beneficial effects of the present invention are as follows: the elongation of 1235D lithium battery aluminum foil can be improved only by adjusting the amount of aluminum-titanium-boron wire added and the cold rolling annealing process, without changing the existing mainstream casting and rolling production process; the obtained lithium battery aluminum foil has a tensile strength of more than 240MPa and an elongation of more than 4.0%, thereby improving the yield rate of the downstream battery industry and the performance stability of lithium-ion batteries. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] The technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiment of the invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional conditions or according to the conditions recommended by the manufacturer. Unless otherwise stated, all percentages, ratios, proportions or parts are by weight. The reagents and raw materials used in the embodiments of the present invention and the comparative examples, if not otherwise specified, can be obtained through commercial channels.
[0033] Example 1
[0034] The chemical composition of a 1235D lithium battery aluminum foil is as follows: Si≤0.04%, Fe: 0.38%, Cu: 0.11%, Mn: 0.02%, Ti: 0.015%, H≤0.10mL / 100gAl, other single impurity elements≤0.03%, and the balance is Al; and the mass percentage of Al is ≥99.35%.
[0035] A method for preparing 1235D lithium battery aluminum foil comprises the following steps:
[0036] Step 1) Ingredients: The ingredients are prepared according to the above-mentioned 1235D lithium battery aluminum foil composition standard, the aluminum ingot raw material used is an electrolytic aluminum ingot with a purity of not less than 99.7%, the addition ratio of cold-rolled secondary scrap is controlled within 5%, and no third-level or above scrap is added;
[0037] Step 2) smelting: placing the raw materials obtained in step 1) in a smelting furnace for smelting, and after the raw materials are melted, refining the obtained aluminum alloy liquid, and adding Fe agent, Cu agent and titanium wire that meet the composition requirements of 1235D lithium battery aluminum foil to obtain aluminum alloy liquid;
[0038] Step 3) insulation: the aluminum alloy liquid obtained in step 2) flows into an insulation furnace for whole furnace refining;
[0039] Step 4) Degassing: Degassing and refining are performed using a degassing box to ensure that the H content in the aluminum liquid is reduced to 0.12mL / 100gAl; and aluminum-titanium-boron wires are added in batches before and after degassing to make the Ti content in the aluminum alloy liquid 0.015% and the B content 0.0015%;
[0040] Step 5) Filtration: The aluminum alloy liquid is subjected to double-stage filtration using a filter box and a ceramic filter plate; the first-stage ceramic filter plate is 50 mesh, the second-stage ceramic filter plate is 60 mesh, and the filtration temperature is 720°C;
[0041] Step 6) Casting and rolling: injecting the aluminum alloy liquid obtained in step 5) into the casting and rolling unit through the flow trough and the front box for continuous casting and rolling to obtain a cast plate with fine and uniform structure;
[0042] Step 7) cold rolling: cold rolling the cast-rolled sheet obtained in step 6) to a thickness of 0.23 mm, and performing intermediate annealing when the thickness is 1.9 mm to refine and homogenize the recrystallized structure, the annealing temperature is 500° C., and the annealing time is 24 hours;
[0043] Step 8) foil rolling: the cold rolled sheet obtained in step 7) is subjected to rough rolling, intermediate rolling and finish rolling to obtain an aluminum foil with a thickness of 0.0013 mm;
[0044] Step 9) Rewind, trim, inspect and package.
[0045] Example 2
[0046] The chemical composition of a 1235D lithium battery aluminum foil is as follows: Si≤0.04%, Fe: 0.38%, Cu: 0.11%, Mn: 0.02%, Ti: 0.020%, H≤0.10mL / 100gAl, other single impurity elements≤0.03%, and the balance is Al; and the mass percentage of Al is ≥99.35%.
[0047] A method for preparing 1235D lithium battery aluminum foil comprises the following steps:
[0048] Step 1) Ingredients: The ingredients are prepared according to the above-mentioned 1235D lithium battery aluminum foil composition standard, the aluminum ingot raw material used is an electrolytic aluminum ingot with a purity of not less than 99.7%, the addition ratio of cold-rolled secondary scrap is controlled within 5%, and no third-level or above scrap is added;
[0049] Step 2) smelting: placing the raw materials obtained in step 1) in a smelting furnace for smelting, and after the raw materials are melted, refining the obtained aluminum alloy liquid, and adding Fe agent, Cu agent and titanium wire that meet the composition requirements of 1235D lithium battery aluminum foil to obtain aluminum alloy liquid;
[0050] Step 3) insulation: the aluminum alloy liquid obtained in step 2) flows into an insulation furnace for whole furnace refining;
[0051] Step 4) Degassing: Degassing and refining are performed using a degassing box to ensure that the H content in the aluminum liquid is reduced to 0.12mL / 100gAl; and aluminum-titanium-boron wires are added in batches before and after degassing to make the Ti content in the aluminum alloy liquid 0.020% and the B content 0.0020%;
[0052] Step 5) Filtration: The aluminum alloy liquid is subjected to double-stage filtration using a filter box and a ceramic filter plate; the first-stage ceramic filter plate is 50 mesh, the second-stage ceramic filter plate is 60 mesh, and the filtration temperature is 721°C;
[0053] Step 6) Casting and rolling: injecting the aluminum alloy liquid obtained in step 5) into the casting and rolling unit through the flow trough and the front box for continuous casting and rolling to obtain a cast plate with fine and uniform structure;
[0054] Step 7) cold rolling: cold rolling the cast-rolled sheet obtained in step 6) to a thickness of 0.23 mm, and performing intermediate annealing when the thickness is 1.9 mm to refine and homogenize the recrystallized structure, the annealing temperature is 500° C., and the annealing time is 24 hours;
[0055] Step 8) foil rolling: the cold rolled sheet obtained in step 7) is subjected to rough rolling, intermediate rolling and finish rolling to obtain an aluminum foil with a thickness of 0.0013 mm;
[0056] Step 9) Rewind, trim, inspect and package.
[0057] Example 3
[0058] The chemical composition of a 1235D lithium battery aluminum foil is as follows: Si≤0.04%, Fe: 0.38%, Cu: 0.11%, Mn: 0.02%, Ti: 0.015%, H≤0.10mL / 100gAl, other single impurity elements≤0.03%, and the balance is Al; and the mass percentage of Al is ≥99.35%.
[0059] A method for preparing 1235D lithium battery aluminum foil comprises the following steps:
[0060] Step 1) Ingredients: The ingredients are prepared according to the above-mentioned 1235D lithium battery aluminum foil composition standard, the aluminum ingot raw material used is an electrolytic aluminum ingot with a purity of not less than 99.7%, the addition ratio of cold-rolled secondary scrap is controlled within 5%, and no third-level or above scrap is added;
[0061] Step 2) smelting: placing the raw materials obtained in step 1) in a smelting furnace for smelting, and after the raw materials are melted, refining the obtained aluminum alloy liquid, and adding Fe agent, Cu agent and titanium wire that meet the composition requirements of 1235D lithium battery aluminum foil to obtain aluminum alloy liquid;
[0062] Step 3) insulation: the aluminum alloy liquid obtained in step 2) flows into an insulation furnace for whole furnace refining;
[0063] Step 4) Degassing: Degassing and refining are performed using a degassing box to ensure that the H content in the aluminum liquid is reduced to 0.12mL / 100gAl; and aluminum-titanium-boron wires are added in batches before and after degassing to make the Ti content in the aluminum alloy liquid 0.015% and the B content 0.0015%;
[0064] Step 5) Filtration: The aluminum alloy liquid is subjected to double-stage filtration using a filter box and a ceramic filter plate; the first-stage ceramic filter plate is 50 mesh, the second-stage ceramic filter plate is 60 mesh, and the filtration temperature is 720°C;
[0065] Step 6) Casting and rolling: injecting the aluminum alloy liquid obtained in step 5) into the casting and rolling unit through the flow trough and the front box for continuous casting and rolling to obtain a cast plate with fine and uniform structure;
[0066] Step 7) cold rolling: cold rolling the cast-rolled sheet obtained in step 6) to a thickness of 0.23 mm, and performing intermediate annealing at a thickness of 1.9 mm to refine and homogenize the recrystallized structure, the annealing temperature being 510° C. and the annealing time being 24 hours;
[0067] Step 8) foil rolling: the cold rolled sheet obtained in step 7) is subjected to rough rolling, intermediate rolling and finish rolling to obtain an aluminum foil with a thickness of 0.0013 mm;
[0068] Step 9) Rewind, trim, inspect and package.
[0069] Comparative Example 1
[0070] The main difference from Example 1 is the Ti content. The specific composition is shown in Table 1 below.
[0071] Comparative Example 2
[0072] The main difference from Example 2 is the annealing temperature. The annealing temperature of Comparative Example 2 is 520° C. The ingredients are shown in Table 1.
[0073] Table 1 Composition of 1235D battery aluminum foil embodiment and comparative example (mass percentage, %)
[0074]
[0075]
[0076] The above Examples 1-3 and Comparative Examples 1-2 were subjected to the following tests, and the test conditions were as follows:
[0077] According to the national standard GB / T 228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method", the tensile strength and elongation of 1235D aluminum foil are tested. The test results are as follows:
[0078]
[0079] From the above table analysis, it can be seen that by adjusting the amount of aluminum titanium boron wire added to adjust the amount of Ti and TiB2 to refine the cast-rolled structure, Ti and B can refine the cast-rolled structure without causing significant TiB2 particle agglomeration and Ti element segregation; on this basis, a suitable cold rolling annealing process is applied to obtain a fine and uniform recrystallized structure, which completes the recrystallization without causing an excessively large recrystallized structure. Therefore, the 1235D battery aluminum foil prepared by the above preparation method of the present invention has a tensile strength of more than 240MPa and an elongation of more than 4.0%, which effectively solves the problem of low elongation of the existing 1235D aluminum foil.
[0080] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A 1235D lithium battery aluminum foil, characterized in that: The chemical composition of the lithium battery aluminum foil, by mass percentage, includes Si≤0.06%, Fe: 0.35%-0.45%, Cu: 0.11%-0.18%, Mn: 0.02%-0.04%, Ti: 0.015%-0.030%, H≤0.12mL / 100gAl, other single impurity elements≤0.03%, and the balance is Al.
2. The 1235D lithium battery aluminum foil according to claim 1, characterized in that: The mass percentage of Al is ≥99.35%.
3. A method for preparing the 1235D lithium battery aluminum foil according to claim 1 or 2, characterized in that: The following steps are involved: Step 1) Ingredients: Ingredients are prepared according to the composition standard of 1235D lithium battery aluminum foil, and the aluminum ingot raw material used is an electrolytic aluminum ingot with a purity of not less than 99.7%; Step 2) smelting: placing the raw materials obtained in step 1) in a smelting furnace for smelting, and after the raw materials are melted, refining the obtained aluminum alloy liquid, and adding alloy materials that meet the composition requirements of 1235D lithium battery aluminum foil to obtain aluminum alloy liquid; Step 3) insulation: the aluminum alloy liquid obtained in step 2) flows into an insulation furnace for whole furnace refining; Step 4) Degassing: Degassing and refining are performed using a degassing box, and aluminum-titanium-boron wires are added in batches before and after degassing, so that the Ti content in the aluminum alloy liquid is 0.015% to 0.030%, and the B content is 0.0015% to 0.0030%; Step 5) Filtration: Using a filter box and a ceramic filter sheet to perform double-stage filtration on the aluminum alloy liquid; Step 6) Casting and rolling: injecting the aluminum alloy liquid obtained in step 5) into the casting and rolling unit through the flow trough, the front box and the casting nozzle for continuous casting and rolling to obtain a cast plate; Step 7) cold rolling: cold rolling the cast-rolled sheet obtained in step 6) to a thickness of 0.20-0.25 mm, and performing intermediate annealing when the thickness is 1.6-2.0 mm to obtain a cold-rolled sheet; Step 8) foil rolling: the cold rolled sheet obtained in step 7) is subjected to rough rolling, intermediate rolling and finish rolling to obtain aluminum foil with a thickness of 0.010-0.015 mm; Step 9) Rewind, trim, inspect and package.
4. The method for preparing 1235D lithium battery aluminum foil according to claim 3, characterized in that: In step 1), the cold-rolled secondary scrap in step 7) is recycled as raw material; wherein the amount of the recycled cold-rolled secondary scrap added is not higher than 5% of the total weight of the aluminum ingot raw material.
5. The method for preparing 1235D lithium battery aluminum foil according to claim 3, characterized in that: In step 2), the refining temperature is 740-750°C.
6. The method for preparing 1235D lithium battery aluminum foil according to claim 3, characterized in that: In step 4), the Ti content of the aluminum titanium boron wire is 4.5%-5.5%, and the B content is 0.8%-1.2%.
7. The method for preparing 1235D lithium battery aluminum foil according to claim 3, characterized in that: In step 5), the double-stage filtration includes a primary ceramic filter plate and a secondary ceramic filter plate; the primary ceramic filter plate is 50 mesh, and the secondary ceramic filter plate is 60 mesh; the filtration temperature is 710°C-730°C.
8. The method for preparing 1235D lithium battery aluminum foil according to claim 3, characterized in that: In step 6), the casting temperature during casting is 688-693° C.; the thickness of the cast plate is 6.5-8.0 mm.
9. The method for preparing 1235D lithium battery aluminum foil according to claim 3, characterized in that: In step 7), the cold rolling is performed in 5 passes, and the distribution scheme of each pass is: (6.5-8.0) mm→(3.2-3.6) mm→(1.6-2.0) mm→(0.6-0.9) mm→(0.3-0.4) mm→(0.20-0.25) mm.
10. The method for preparing 1235D lithium battery aluminum foil according to claim 3, characterized in that: In step 7), the intermediate annealing conditions are: the annealing furnace gas temperature is 480-530° C., the temperature is kept for 20-25 hours, and then the mixture is air-cooled to room temperature.