Thermal oxide layer after magnetron sputtering of pre-deposition layer on titanium alloy surface and preparation method
By adding a pre-deposition layer to the surface of the titanium alloy and undergoing magnetron sputtering and thermal oxidation treatment, a dense oxide layer is formed, which solves the problems of discontinuity and fall off of the oxide layer in the prior art, and significantly improves the friction on the surface of the titanium alloy and corrosion performance.
Patent Information
- Application Number
- CN202411248970.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing surface thermal oxidation technology of titanium alloys, insufficient temperature and time lead to discontinuous oxide formation, coating and substrate fall off, insufficient friction and corrosion performance, affecting the service life of the implant.
First, pre-deposition layers such as Ag, Ta, Cr, etc. are added to the surface of the titanium alloy, and then magnetron sputtering and thermal oxidation are performed to determine the optimal thermal oxidation parameters to form a dense and uniform oxide layer.
Significantly increase the thickness and density of the oxide layer, improve the friction and corrosion performance of the surface of titanium alloy, and extend the service life of the implant.
Smart Images

Figure CN119040790A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal surface treatment, and in particular relates to a titanium alloy surface magnetron sputtering pre-deposition layer followed by a thermal oxidation layer and a preparation method thereof. Background Art
[0002] Titanium and titanium alloys have become the preferred materials for biomedical products due to their low density, low toxicity, excellent corrosion resistance and biocompatibility. However, compared with human tissue, titanium implants are still a kind of foreign material. After titanium and its titanium alloys are implanted in the body, they first interact with the surrounding environment through the surface. Their surface morphology and structure have a great influence on the implant effect, and to a large extent determine whether the implant can combine with human tissue and perform its function. Therefore, the surface treatment technology of titanium alloys has received the focus of attention of researchers at home and abroad. By modifying the surface of titanium alloys, it is possible to prevent the wear of artificial joints during long-term use, reduce the generation of abrasive particles, and thus extend the service life of artificial joints and other human tissues.
[0003] A large number of studies have shown that the TiO2 oxide layer formed spontaneously by thermal oxidation can improve the friction and corrosion properties of titanium alloys in the human body. However, insufficient temperature and time may lead to the formation of discontinuous oxides. High temperature and long time will lead to the peeling between the coating and the substrate. Summary of the invention
[0004] In order to overcome the problems existing in the related art, the disclosed embodiment of the present invention provides a titanium alloy surface magnetron sputtering pre-deposition layer and a thermal oxidation layer and a preparation method. The purpose of the present invention is to improve the friction performance of thin or thick oxide layers. The method of adding a pre-deposition layer to the titanium alloy surface and then thermally oxidizing it is analyzed, and the influence mechanism of the pre-deposition layer on the oxide layer formed by thermal oxidation is analyzed. The present invention selects Ag, Ta, and Cr as the pre-deposition layer before thermal oxidation.
[0005] The technical scheme is as follows: A method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface, comprising:
[0006] S1, subjecting the titanium alloy to thermal oxidation treatment at different temperatures and for different times to determine the optimal thermal oxidation parameters;
[0007] S2, preparing Ag, Ta, and Cr pre-deposition layers of different thicknesses on the titanium alloy surface by magnetron sputtering;
[0008] S3, placing the titanium alloy with the pre-deposition layer into a tube furnace, performing thermal oxidation treatment of TOAg, TOTa, and TOCr, and obtaining an oxide layer on the surface of the titanium alloy.
[0009] In step S1, the titanium alloy is subjected to thermal oxidation treatment at different temperatures and for different times, including the following steps:
[0010] Sample processing;
[0011] Thermal oxidation temperature selection: thermal oxidation treatment of titanium alloy at different temperatures;
[0012] Thermal oxidation time selection: thermal oxidation treatment of titanium alloy at different times;
[0013] Thermal oxidation parameters are determined by selecting thermal oxidation temperature and thermal oxidation time.
[0014] Further, the sample processing includes: cutting a 6mm diameter TC4 rod into a 20mm long cylinder, then cutting off 1mm thickness at the top and bottom to cut out a friction sample that is conducive to the test of friction performance, grinding the cut sample with 240-7000 mesh sandpaper, and polishing with diamond polishing paste; then using alcohol ultrasonic treatment for 15 minutes to dry the polished sample for later use;
[0015] The thermal oxidation temperature selection includes: thermally oxidizing the titanium alloy at 550°C, 600°C, 650°C, and 700°C for 10 hours respectively; the thickness of the generated oxide layer is 1.82μm, 2.45μm, 3.1μm, and 4.9μm respectively;
[0016] The thermal oxidation time selection includes: determining 650° C. by thermal oxidation temperature selection, and performing thermal oxidation treatment on the titanium alloy at 650° C. for 1 h, 5 h, 10 h, 20 h, and 40 h, respectively; the thickness of the generated oxide layer is 1.94 μm, 2.72 μm, 3.7 μm, and 4.5 μm, respectively;
[0017] The thermal oxidation parameters are determined according to the thermal oxidation temperature and thermal oxidation time as thermal oxidation at 650°C for 10 hours.
[0018] In step S2, Ag, Ta, and Cr pre-deposition layers of different thicknesses are prepared, including: target replacement, vacuuming, film coating, and thermal oxidation.
[0019] In step S3, TOAg and TOTa are thermally oxidized, including:
[0020] Sample processing: Cut the TC4 rod with a diameter of 6mm into a cylinder with a length of 20mm, and then cut off 1mm thickness on the top and bottom to cut out the friction sample for the test of friction performance. Grind the cut sample with 240-7000 mesh sandpaper, and then polish it with diamond polishing paste; then use alcohol ultrasonic for 15 minutes, and then blow dry for use;
[0021] TOAg, TOTa sputtering pre-deposition layer: put the titanium alloy into a multi-target magnetron sputtering instrument, rotate the sample stage to the top of the Ag target or Ta target through computer control, and obtain Ag and Ta layers of different thicknesses on the surface of the titanium alloy by adjusting the magnetron sputtering power;
[0022] TOAg, TOTa thermal oxidation treatment: The titanium alloy pre-deposited with Ag and Ta layers is placed in a tube furnace for thermal oxidation treatment.
[0023] Furthermore, in the TOAg and TOTa sputtering pre-deposition step, the rotation speed was controlled to 3.8 rps and the vacuum degree of the sample chamber reached 4×10 -3 After Pa, 15 sccm of Ar was introduced into the cavity; the powers of magnetron sputtering were 30 W, 50 W, and 70 W, respectively; the thicknesses of the sputtered Ag layer on the sample surface were 1.25 μm, 1.88 μm, and 2.95 μm, respectively, and the thicknesses of the sputtered Ta layer on the sample surface were 251.7 nm, 781.7 nm, and 1.05 μm, respectively.
[0024] Furthermore, in the TOAg and TOTa thermal oxidation treatment steps, the thermal oxidation parameters were 650°C thermal oxidation for 10 hours; the thickness of the oxide layer after TOAg treatment was 22.1 μm, 12.2 μm, and 14.1 μm, respectively; the thickness of the oxide layer after TOTa treatment was 5.8 μm, 4.8 μm, and 2.8 μm, respectively.
[0025] In step S3, the TOCr thermal oxidation treatment includes:
[0026] Sample processing: Cut the 6mm diameter TC4 rod into a 20mm long cylinder and then cut off 1mm thickness on the top and bottom to cut out the friction test sample that is beneficial to the friction performance. Grind the cut sample with 240-7000 mesh sandpaper and polish it with diamond polishing paste. Use alcohol ultrasonic treatment for 15 minutes to dry the polished sample for later use.
[0027] TOCr sputtering pre-deposition layer: The titanium alloy is placed in a CF-800 unbalanced closed field magnetron sputtering ion plating system, and by adjusting the magnetron sputtering parameters, a Cr layer of different thicknesses is obtained on the surface of the titanium alloy;
[0028] TOCr thermal oxidation treatment: The titanium alloy with a pre-deposited Cr layer is placed in a tube furnace for thermal oxidation treatment.
[0029] Furthermore, in the TOCr sputtering pre-deposition layer step, the deposition parameters are: the coating is carried out in an argon environment, the target material is a Cr target, the current is 1A, and the bias voltage is 40V; the frequency of the pulse mode is 50kHz, and the pulse width is 1500ns; the deposition time of the coating is 1h, 1.5h, 3h, and 6h respectively; the thickness of the Cr layer sputtered on the sample surface by different processes is 361.3nm, 457.5nm, 1.01μm, and 2.15μm respectively;
[0030] In the TOCr thermal oxidation treatment step, the thermal oxidation parameters are 650°C thermal oxidation for 10 hours; the thicknesses of the thermal oxidation layers after TOCr treatment are 2.5 μm, 10.0 μm, 18.0 μm, and 28.0 μm, respectively.
[0031] Another object of the present invention is to provide a titanium alloy surface magnetron sputtering pre-deposition layer followed by thermal oxidation layer, which is prepared using the titanium alloy surface magnetron sputtering pre-deposition layer followed by thermal oxidation layer preparation method.
[0032] In combination with all the above technical solutions, the beneficial effects of the present invention are as follows: the present invention studies the influence of thermal oxidation process parameters on the microstructure and friction performance of titanium alloy by subjecting titanium alloy to thermal oxidation treatment (TO) at different temperatures and for different times. Then, based on the study of thermal oxidation treatment of titanium alloy, Ag, Ta, and Cr pre-deposition layers of different thicknesses are deposited on the surface of titanium alloy by magnetron sputtering, and then subjected to thermal oxidation treatment (TOAg, TOTa, TOCr), and the influence of pre-deposition layers of different thicknesses on the microstructure and performance of the oxide layer formed by thermal oxidation is analyzed. In the present invention, a dense and uniform oxide layer is formed on the surface of titanium alloy by magnetron sputtering the pre-deposition layer and then thermally oxidizing it, which can significantly increase the thickness of the oxide layer and improve the friction and corrosion properties of the titanium alloy surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The accompanying drawings herein are incorporated in and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the description, serve to explain the principles of the present disclosure;
[0034] Figure 1 It is a flow chart of a method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface provided by an embodiment of the present invention;
[0035] Figure 2 It is a schematic diagram of a method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface provided by an embodiment of the present invention;
[0036] Figure 3 It is a surface morphology diagram of four groups of cases of thermal oxidation treatment of TO, TOAg, TOTa and TOC provided in the embodiments of the present invention;
[0037] Figure 4 It is a cross-sectional morphology diagram of Examples 2, 3, 4 and Comparative Example 1 provided in the embodiments of the present invention;
[0038] Figure 5 It is a friction depth diagram of Examples 2, 3, 4 and Comparative Example 1 provided in the embodiments of the present invention;
[0039] Figure 6 It is a friction morphology diagram of Examples 2, 3, 4 and Comparative Example 1 provided in the embodiments of the present invention;
[0040] Figure 7 It is a polarization curve diagram of Examples 2, 3, 4 and Comparative Example 1 provided in the embodiments of the present invention. DETAILED DESCRIPTION
[0041] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.
[0042] The innovation of the present invention is that the thermal oxidation layer on the surface of the titanium alloy is composed of the oxide of the pre-deposition layer, the pre-deposition layer elements and TiO2. The addition of the pre-deposition layer promotes the diffusion of Ti and O, and increases the thickness of the oxide layer on the surface of the titanium alloy. The present invention first performs different thermal oxidation times and different thermal oxidation temperatures on the surface of the titanium alloy to obtain the best thermal oxidation parameters, and then performs thermal oxidation treatment after the pre-deposition layer is deposited on the surface of the titanium alloy using a magnetron sputtering device. A thermal oxidation layer with uniform particle distribution and good compactness is obtained, thereby improving the wear resistance and corrosion resistance of the titanium alloy surface.
[0043] like Figure 1 As shown, the method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface provided by the present invention comprises:
[0044] S1, subjecting the titanium alloy to thermal oxidation treatment at different temperatures and for different times to determine the optimal thermal oxidation parameters;
[0045] S2, preparing Ag, Ta, and Cr pre-deposition layers of different thicknesses on the titanium alloy surface by magnetron sputtering;
[0046] S3, placing the titanium alloy with the pre-deposition layer into a tube furnace, performing thermal oxidation treatment of TOAg, TOTa, and TOCr, and obtaining an oxide layer on the surface of the titanium alloy.
[0047] In step S1, the thermal oxidation treatment of TO at different temperatures and for different times includes the following steps:
[0048] Sample processing: Cut the 6mm diameter TC4 rod into a 20mm long cylinder and cut off 1mm thickness on the top and bottom to cut out a larger platform to facilitate the test of friction performance. Therefore, the size of the friction sample is a block with a length of 20mm and a thickness of 4mm. Grind the cut sample with 240-7000 mesh sandpaper, and then polish it with diamond polishing paste. Then use alcohol ultrasound for 15 minutes, and then blow dry for use.
[0049] Thermal oxidation temperature selection: The titanium alloy was thermally oxidized at 550℃, 600℃, 650℃, and 700℃ for 10h respectively; the thickness of the generated oxide layer was 1.82μm, 2.45μm, 3.1μm, and 4.9μm respectively. The wear rates were: 5.98×10 - 4 mm 3 N -1 ·m -1 , 2.7×10 -5 mm 3 N -1 ·m -1 , 2.6×10 -6 mm 3 N -1 ·m -1 , 6.5×10 -5 mm 3 N -1 ·m -1 .
[0050] Thermal oxidation time selection: The thermal oxidation temperature was determined to be 650℃, and the titanium alloy was thermally oxidized at 650℃ for 1h, 5h, 10h, 20h, and 40h respectively; the thickness of the generated oxide layer was 1.94μm, 2.72μm, 3.7μm, and 4.5μm respectively. The wear rates were 6.78×10 -4 mm 3 N -1 ·m -1 , 6.13×10 -4 mm 3 N -1 ·m -1 , 2.6×10 -6 mm 3 N -1 ·m -1 , 5.2×10 -5 mm 3 N -1 ·m -1 , 6.6×10 -5 mm 3 N-1 ·m -1 .
[0051] The optimal thermal oxidation parameters were determined to be thermal oxidation at 650°C for 10 hours based on the thermal oxidation temperature and thermal oxidation time.
[0052] In step S3, the TOAg and TOTa thermal oxidation treatment method includes the following steps:
[0053] Sample processing: Cut the 6mm diameter TC4 rod into a 20mm long cylinder and cut off 1mm thickness on the top and bottom to cut out a larger platform to facilitate the test of friction performance. Therefore, the size of the friction sample is a block with a length of 20mm and a thickness of 4mm. Grind the cut sample with 240-7000 mesh sandpaper, and then polish it with diamond polishing paste. Then use alcohol ultrasound for 15 minutes, and then blow dry for use.
[0054] TOAg, TOTa sputtering pre-deposition layer: Put the titanium alloy into the JGP-450 multi-target magnetron sputtering instrument, rotate the sample stage to the top of the Ag target or Ta target through computer control, and obtain Ag and Ta layers of different thicknesses on the surface of the titanium alloy by adjusting the magnetron sputtering power;
[0055] TOAg, TOTa thermal oxidation treatment: The titanium alloy pre-deposited with Ag and Ta layers is placed in a tube furnace for thermal oxidation treatment.
[0056] In the embodiment of the present invention, in the step of sputtering the pre-deposition layer of TOAg and TOTa, the rotation speed is controlled to be 3.8 rps, and the vacuum degree of the sample chamber reaches 4×10 -3 After Pa, 15sccm of Ar was introduced into the chamber. The powers of magnetron sputtering were 30W, 50W, and 70W respectively. The thickness of the sputtered Ag layer on the sample surface was about 1.25μm, 1.88μm, and 2.95μm respectively, and the thickness of the sputtered Ta layer on the sample surface was about 251.7nm, 781.7nm, and 1.05μm respectively.
[0057] In the embodiment of the present invention, in the TOAg and TOTa thermal oxidation treatment steps, the thermal oxidation parameters are 650°C thermal oxidation for 10 hours. The thickness of the oxide layer after TOAg treatment is 22.1 μm, 12.2 μm, and 14.1 μm respectively. The thickness of the oxide layer after TOTa treatment is 5.8 μm, 4.8 μm, and 2.8 μm respectively.
[0058] In an embodiment of the present invention, the TOCr thermal oxidation treatment method comprises the following steps:
[0059] Sample processing: Cut the 6mm diameter TC4 rod into a 20mm long cylinder and cut off 1mm thickness on the top and bottom to cut out a larger platform to facilitate the test of friction performance. Therefore, the size of the friction sample is a block with a length of 20mm and a thickness of 4mm. Grind the cut sample with 240-7000 mesh sandpaper, and then polish it with diamond polishing paste. Then use alcohol ultrasound for 15 minutes, and then blow dry for use.
[0060] TOCr sputtering pre-deposition layer: The titanium alloy is placed in a CF-800 unbalanced closed field magnetron sputtering ion plating system, and by adjusting the magnetron sputtering parameters, a Cr layer of different thicknesses is obtained on the surface of the titanium alloy;
[0061] TOCr thermal oxidation treatment: The titanium alloy with a pre-deposited Cr layer is placed in a tube furnace for thermal oxidation treatment.
[0062] In the TOCr sputtering pre-deposition layer step, the deposition parameters are: Deposition parameters: The coating is carried out in an argon environment, the target material is a Cr target, the current is 1A, and the bias voltage is 40V. The frequency of the pulse mode is 50kHz, and the pulse width is 1500ns. The deposition time of the coating is 1h, 1.5h, 3h, and 6h respectively. The thickness of the Cr layer sputtered on the sample surface with different processes is 361.3nm, 457.5nm, 1.01μm, and 2.15μm respectively.
[0063] In the TOCr thermal oxidation treatment step, the thermal oxidation parameters are 650°C thermal oxidation for 10 hours. The thicknesses of the thermal oxidation layers after TOCr treatment are 2.5 μm, 10.0 μm, 18.0 μm, and 28.0 μm, respectively.
[0064] It can be seen from the above embodiments that the present invention can significantly increase the thickness of the thermal oxidation layer and improve the friction and corrosion properties of the titanium alloy surface. Compared with the prior art, the present invention first performs thermal oxidation at different temperatures and for different times to obtain the best thermal oxidation parameters. The oxide layer obtained by this treatment is relatively thin, and the thickness of the generated oxide layer is as thick as about 5μm. The interaction between rutile TiO2 and anatase TiO2 can improve the surface hardness of the titanium alloy and increase the wear resistance and corrosion resistance. Then, by thermal oxidation treatment after the pre-deposition layer on the surface of the titanium alloy, the oxide of the deposition layer and TiO2 are mutually embedded to form a thicker thermal oxidation layer, and the thickness of the oxide layer can reach more than 20μm. The compactness and size uniformity of the thermal oxidation layer after the pre-deposition layer of the present invention are better than the thermal oxidation layer formed by simple thermal oxidation. Therefore, magnetron sputtering the pre-deposition layer on the titanium alloy and then performing thermal oxidation can further improve the friction and corrosion properties compared with simple thermal oxidation treatment.
[0065] The embodiment of the present invention also provides a titanium alloy surface magnetron sputtering pre-deposition layer followed by thermal oxidation layer prepared according to the method for preparing a titanium alloy surface magnetron sputtering pre-deposition layer followed by thermal oxidation layer.
[0066] in Figure 2 The invention discloses the principle of the preparation method of the thermal oxidation layer after the magnetron sputtering pre-deposition layer on the titanium alloy surface.
[0067] Comparative Example 1: The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface provided in the prior art of the present invention comprises the following steps:
[0068] Sample processing: Cut the 6mm diameter TC4 rod into a 20mm long cylinder and cut off 1mm thickness on the top and bottom to cut out a larger platform to facilitate the test of friction performance. Therefore, the size of the friction sample is a block with a length of 20mm and a thickness of 4mm. Grind the cut sample with 240-7000 mesh sandpaper, and then polish it with diamond polishing paste. Then use alcohol ultrasound for 15 minutes, and then blow dry for use.
[0069] Thermal oxidation temperature selection: The treated titanium alloy is placed in a tube furnace and subjected to thermal oxidation treatment at 550°C, 600°C, 650°C, and 700°C for 10 hours respectively. The surface microstructure and cross-sectional morphology of the thermally oxidized titanium alloy are characterized, and its friction and corrosion properties are tested to determine the optimal thermal oxidation temperature;
[0070] Thermal oxidation time selection: 650°C was selected as the thermal oxidation temperature, and the titanium alloy was thermally oxidized at 650°C for 1h, 5h, 10h, 20h, and 40h. The surface micromorphology and cross-sectional morphology of the thermally oxidized titanium alloy were characterized, and its friction and corrosion properties were tested.
[0071] Optimal thermal oxidation parameters: Based on the thermal oxidation temperature and thermal oxidation time, the optimal thermal oxidation parameters were determined to be thermal oxidation at 650°C for 10 hours.
[0072] Embodiment 2, the method for preparing a thermal oxidation layer after pre-depositing an Ag layer on a titanium alloy surface by magnetron sputtering provided in the embodiment of the present invention specifically comprises the following steps:
[0073] S1: sample pretreatment;
[0074] S2: magnetron sputtering Ag layer to obtain Ag layers of different thicknesses;
[0075] S3: Thermal oxidation treatment of the titanium alloy with the deposited Ag layer
[0076] S4: Obtain thermal oxide layers of different thicknesses.
[0077] In the sample pretreatment step, the TC4 rod with a diameter of 6mm was cut into a cylinder with a length of 20mm, and then 1mm thickness was cut off at the top and bottom to cut out a larger platform to facilitate the test of friction performance. Therefore, the size of the friction sample is a block with a length of 20mm and a thickness of 4mm. The cut sample was ground with sandpaper and then polished with polishing paste. The polished sample was then ultrasonicated with alcohol for 15 minutes, and then blown dry for use.
[0078] The sandpaper described in step S1 of the embodiment of the present invention has mesh sizes of 240, 400, 800, 100, 1500, 2000, 3000, 5000, and 700 respectively;
[0079] The polishing paste described in step S1 of the embodiment of the present invention is a diamond polishing paste with a particle size of W1.5.
[0080] In step S2 of the embodiment of the present invention, the magnetron sputtering Ag layer comprises:
[0081] S201, target change: the Ag layer was deposited by a JGP-450 multi-target magnetron sputtering instrument (Shenyang Scientific Instrument Co., Ltd., Chinese Academy of Sciences). An Ag target with a diameter of 75 mm and a thickness of 3 mm was placed at the cathode of the DC power supply, and the sample compartment door was closed;
[0082] S202, vacuum: close the vent valve, turn on the mechanical pump, wait until the air pressure drops to 8-9Pa, then open the solenoid valve, turn on the molecular pump, and wait until the vacuum reaches 4×10 -3 Pa;
[0083] S203, coating: press the function key, open the Ar ventilation valve, then turn on the gas flow switch, turn on the main power switch, turn on the turntable motor switch, the self-rotating motor, and the DC power supply, turn on the Ar flow rate to 30sccm, adjust the gas pressure to 2-4Pa, wait for a while, adjust the Ar flow rate to 15sccm, adjust the DC power supply power, adjust the gas pressure to 0.5Pa, and sputter for 30min;
[0084] S301, thermal oxidation: put the titanium alloy deposited with the Ag layer into a tube furnace, let in air, maintain a heating rate of 10°C / min, raise the temperature to 650°C, keep the temperature for 10 hours, then end the program and let the sample cool down with the furnace.
[0085] In step S203 of the embodiment of the present invention, the DC power supply powers are 30W, 50W, and 70W respectively.
[0086] Embodiment 3, the method for preparing a thermal oxidation layer after magnetron sputtering pre-deposition of a Ta layer on a titanium alloy surface provided in the embodiment of the present invention specifically comprises the following steps:
[0087] S1: sample pretreatment;
[0088] S2: magnetron sputtering Ta layer to obtain Ta layer of different thickness;
[0089] S3: thermally oxidizing the titanium alloy having the deposited Ta layer;
[0090] S4: Obtain thermal oxide layers of different thicknesses.
[0091] In the sample pretreatment step, the TC4 rod with a diameter of 6mm was cut into a cylinder with a length of 20mm, and then 1mm thickness was cut off at the top and bottom to cut out a larger platform to facilitate the test of friction performance. Therefore, the size of the friction sample is a block with a length of 20mm and a thickness of 4mm. The cut sample was ground with sandpaper and then polished with polishing paste. The polished sample was then ultrasonicated with alcohol for 15 minutes, and then blown dry for use.
[0092] The sandpaper described in step S1 of the embodiment of the present invention has mesh sizes of 240, 400, 800, 100, 1500, 2000, 3000, 5000, and 700 respectively;
[0093] The polishing paste described in step S1 of the embodiment of the present invention is a diamond polishing paste with a particle size of W1.5.
[0094] In step S2 of the embodiment of the present invention, the magnetron sputtering Ta layer comprises:
[0095] S201, target change: Ta layer was deposited by JGP-450 multi-target magnetron sputtering instrument (Shenyang Scientific Instrument Co., Ltd., Chinese Academy of Sciences), and an Ag target with a diameter of 75 mm and a thickness of 3 mm was placed at the cathode of the DC power supply, and the sample compartment door was closed;
[0096] S202, vacuum: close the vent valve, turn on the mechanical pump, wait until the air pressure drops to 8-9Pa, then open the solenoid valve, turn on the molecular pump, and wait until the vacuum reaches 4×10 -3 Pa;
[0097] S203, coating: press the function key, open the Ar ventilation valve, then turn on the gas flow switch, turn on the main power switch, turn on the turntable motor switch, the self-rotating motor, and the DC power supply, turn on the Ar flow rate to 30sccm, adjust the gas pressure to 2-4Pa, wait for a while, adjust the Ar flow rate to 15sccm, adjust the DC power supply power, adjust the gas pressure to 0.5Pa, and sputter for 30min;
[0098] S301, thermal oxidation: put the titanium alloy deposited with Ta layer into a tubular furnace, let in air, maintain the heating rate at 10℃ / min, raise the temperature to 650℃, keep the temperature for 10h, then end the program and let the sample cool down with the furnace.
[0099] In step S203 of the embodiment of the present invention, the DC power supply power is 30W, 50W, and 70W respectively.
[0100] Embodiment 4, the method for preparing a thermal oxidation layer after magnetron sputtering pre-deposition of a Cr layer on the titanium alloy surface provided in the embodiment of the present invention specifically comprises the following steps:
[0101] S1: sample pretreatment;
[0102] S2: magnetron sputtering Cr layer to obtain Cr layer with different thickness;
[0103] S3: thermally oxidizing the titanium alloy having the deposited Cr layer;
[0104] S4: Obtain thermal oxide layers of different thicknesses.
[0105] In the sample pretreatment step, the TC4 rod with a diameter of 6mm was cut into a cylinder with a length of 20mm, and then 1mm thickness was cut off at the top and bottom to cut out a larger platform to facilitate the test of friction performance. Therefore, the size of the friction sample is a block with a length of 20mm and a thickness of 4mm. The cut sample was ground with sandpaper and then polished with polishing paste. The polished sample was then ultrasonicated with alcohol for 15 minutes, and then blown dry for use.
[0106] The sandpaper described in step S1 of the embodiment of the present invention has mesh sizes of 240, 400, 800, 100, 1500, 2000, 3000, 5000, and 700 respectively;
[0107] The polishing paste described in step S1 of the embodiment of the present invention is a diamond polishing paste with a particle size of W1.5.
[0108] In step S2 of the embodiment of the present invention, the magnetron sputtering Cr layer comprises:
[0109] S201, target change: The Cr layer is deposited by the CF-800 non-equilibrium closed field magnetron sputtering ion plating system designed and produced by the British TEER company. The size of the Cr target is 470×145×8mm. Turn on the magnetron sputtering equipment switch, then turn on the air compressor and cooling water, then return to the screen and press On, then click startup to turn hold to cold, wait for acclerating at the top of the screen to turn to ready, click vent to deflate, open the sample chamber door, and install the target material on the Cu backing plate with good thermal conductivity. Put the titanium alloy on the sample rack;
[0110] S202, vacuum: Close the sample chamber door and click pump down to wait for the vacuum to reach 3×10 -5 Pa;
[0111] S203, coating: open startprocess, set sputtering process parameters, start coating, after coating is completed, click standby and then click vent to open the door for sampling;
[0112] S301, thermal oxidation: put the titanium alloy deposited with Ta layer into a tubular furnace, let in air, maintain the heating rate at 10℃ / min, raise the temperature to 650℃, keep the temperature for 10h, then end the program and let the sample cool down with the furnace.
[0113] In step S203 of the embodiment of the present invention, the sputtering process parameters are: the coating is carried out in an argon environment, the target material is a Cr target, the current is 1A, the bias voltage is 40V, the frequency of the pulse mode is 50kHz, and the pulse width is 1500ns. The deposition time of the coating is 1h, 1.5h, 3h, and 6h respectively.
[0114] in, Figure 3 It is a surface morphology diagram of four groups of cases of thermal oxidation treatment of TO, TOAg, TOTa and TOCr provided in the embodiments of the present invention; Figure 4 It is a cross-sectional morphology diagram of Examples 2, 3, 4 and Comparative Example 1 provided in the embodiments of the present invention; Figure 5 It is a friction depth diagram of Examples 2, 3, 4 and Comparative Example 1 provided in the embodiments of the present invention; Figure 6 It is a friction morphology diagram of Examples 2, 3, 4 and Comparative Example 1 provided in the embodiments of the present invention; Figure 7 It is a polarization curve diagram of Examples 2, 3, 4 and Comparative Example 1 provided in the embodiments of the present invention.
[0115] Performance test: Performance tests were performed on Examples 2, 3, 4 and Comparative Example 1. The hardness of the alloy was measured using a Vickers hardness tester (VHS-1000); the surface micromorphology and cross-sectional morphology of the oxide layer were characterized in the experiment using a QuantaFEG450 field emission environmental scanning electron microscope (Scanning electron microscopy, SEM); the tribological performance test of the coating was completed using an MFT-5000 multifunctional friction and wear tester; the corrosion performance was tested using Shanghai Chenhua Instrument CHI600; the results are shown in Table 1.
[0116] Table 1 Performance test table
[0117] Section thickness (μm) Hardness (HV) Friction depth (μm) <![CDATA[Corrosion current density (A / cm 2 )]]> Comparative Example 1 4.5 937.8 1.64 <![CDATA[1.19×10 -5 <!-- 7 -->]]> Comparative Example 2 22.1 522.2 0.68 <![CDATA[1.263×10 -6 ]]> Comparative Example 3 5.8 1010.8 0.28 <![CDATA[2.26×10 -6 ]]> Comparative Example 4 28 750.0 0.31 <![CDATA[2.47×10 -9 ]]>
[0118] As can be seen from Table 1, compared with the simple thermal oxidation treatment, after the pre-deposition layer on the titanium alloy surface, the thermal oxidation treatment was performed at 650℃ / 10h. Due to the presence of the deposited layer elements, the vacancy diffusion of O was promoted, and more O combined with Ti to form a dense TiO2 layer, and its thickness increased significantly. At the same time, due to the mutual embedding of the oxide of the pre-deposition layer and the TiO2 particles, the wear resistance of the oxide of the deposition layer interacted with the high hardness of TiO2, which improved the friction performance. The addition of the pre-deposition layer makes the surface oxide layer of the titanium alloy more uniform, the friction coefficient is reduced, the friction depth is increased, and the corrosion current density is reduced.
[0119] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0120] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principles of the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing a thermal oxidation layer on a titanium alloy surface after magnetron sputtering pre-deposition layer, It is characterized in that The preparation method comprises: S1, subjecting the titanium alloy to thermal oxidation treatment at different temperatures and for different times to determine the optimal thermal oxidation parameters; S2, preparing Ag, Ta, and Cr pre-deposition layers of different thicknesses on the titanium alloy surface by magnetron sputtering; S3, placing the titanium alloy with the pre-deposition layer into a tube furnace, performing thermal oxidation treatment of TOAg, TOTa, and TOCr, and obtaining an oxide layer on the surface of the titanium alloy.
2. The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface according to claim 1, It is characterized in that In step S1, the titanium alloy is subjected to thermal oxidation treatment at different temperatures and for different times, including the following steps: Sample processing; Thermal oxidation temperature selection: thermal oxidation treatment of titanium alloy at different temperatures; Thermal oxidation time selection: thermal oxidation treatment of titanium alloy at different times; Thermal oxidation parameters are determined by selecting thermal oxidation temperature and thermal oxidation time.
3. The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface according to claim 2, It is characterized in that The sample processing includes: cutting a 6mm diameter TC4 rod into a 20mm long cylinder, then cutting off 1mm thickness at the top and bottom to cut out a friction sample that is conducive to the test of friction performance, grinding the cut sample with 240-7000 mesh sandpaper, and polishing with diamond polishing paste; then using alcohol ultrasonic treatment for 15 minutes to dry the polished sample for later use; The thermal oxidation temperature selection includes: thermally oxidizing the titanium alloy at 550°C, 600°C, 650°C, and 700°C for 10 hours respectively; the thickness of the generated oxide layer is 1.82 μm, 2.45 μm, 3.1 μm, and 4.9 μm respectively; The thermal oxidation time selection includes: determining 650° C. by thermal oxidation temperature selection, and performing thermal oxidation treatment on the titanium alloy at 650° C. for 1 h, 5 h, 10 h, 20 h, and 40 h, respectively; the thickness of the generated oxide layer is 1.94 μm, 2.72 μm, 3.7 μm, and 4.5 μm, respectively; The thermal oxidation parameters are determined according to the thermal oxidation temperature and thermal oxidation time as thermal oxidation at 650°C for 10 hours.
4. The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface according to claim 1, It is characterized in that In step S2, Ag, Ta, and Cr pre-deposition layers of different thicknesses are prepared, including: target replacement, vacuuming, film coating, and thermal oxidation.
5. The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface according to claim 1, It is characterized in that In step S3, TOAg and TOTa are thermally oxidized, including: Sample processing: Cut the TC4 rod with a diameter of 6mm into a cylinder with a length of 20mm, and then cut off 1mm thickness on the top and bottom to cut out the friction sample for the test of friction performance. Grind the cut sample with 240-7000 mesh sandpaper, and then polish it with diamond polishing paste; then use alcohol ultrasonic for 15 minutes, and then blow dry for use; TOAg, TOTa sputtering pre-deposition layer: put the titanium alloy into a multi-target magnetron sputtering instrument, rotate the sample stage to the top of the Ag target or Ta target through computer control, and obtain Ag and Ta layers of different thicknesses on the surface of the titanium alloy by adjusting the magnetron sputtering power; TOAg, TOTa thermal oxidation treatment: The titanium alloy pre-deposited with Ag and Ta layers is placed in a tube furnace for thermal oxidation treatment.
6. The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface according to claim 5, It is characterized in that In the TOAg and TOTa sputtering pre-deposition step, the rotation speed was controlled to 3.8 rps and the vacuum degree of the sample chamber reached 4×10 -3 After Pa, 15 sccm of Ar was introduced into the cavity; the powers of magnetron sputtering were 30 W, 50 W, and 70 W, respectively; the thicknesses of the sputtered Ag layer on the sample surface were 1.25 μm, 1.88 μm, and 2.95 μm, respectively, and the thicknesses of the sputtered Ta layer on the sample surface were 251.7 nm, 781.7 nm, and 1.05 μm, respectively.
7. The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface according to claim 5, It is characterized in that In the TOAg and TOTa thermal oxidation treatment steps, the thermal oxidation parameters are 650°C thermal oxidation for 10 hours; the thickness of the oxide layer after TOAg treatment is 22.1μm, 12.2μm, and 14.1μm, respectively; the thickness of the oxide layer after TOTa treatment is 5.8μm, 4.8μm, and 2.8μm, respectively.
8. The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface according to claim 1, It is characterized in that In step S3, the TOCr thermal oxidation treatment includes: Sample processing: Cut the 6mm diameter TC4 rod into a 20mm long cylinder and then cut off 1mm thickness on the top and bottom to cut out the friction test sample that is beneficial to the friction performance. Grind the cut sample with 240-7000 mesh sandpaper and polish it with diamond polishing paste. Use alcohol ultrasonic treatment for 15 minutes to dry the polished sample for later use. TOCr sputtering pre-deposition layer: The titanium alloy is placed in a CF-800 unbalanced closed field magnetron sputtering ion plating system, and by adjusting the magnetron sputtering parameters, a Cr layer of different thicknesses is obtained on the surface of the titanium alloy; TOCr thermal oxidation treatment: The titanium alloy with a pre-deposited Cr layer is placed in a tube furnace for thermal oxidation treatment.
9. The method for preparing a thermal oxidation layer after a magnetron sputtering pre-deposition layer on a titanium alloy surface according to claim 8, It is characterized in that In the TOCr sputtering pre-deposition layer step, the deposition parameters are: the coating is carried out in an argon environment, the target material is a Cr target, the current is 1A, and the bias voltage is 40V; the frequency of the pulse mode is 50kHz, and the pulse width is 1500ns; the deposition time of the coating is 1h, 1.5h, 3h, and 6h respectively; the thickness of the Cr layer sputtered on the sample surface by different processes is 361.3nm, 457.5nm, 1.01μm, and 2.15μm respectively; In the TOCr thermal oxidation treatment step, the thermal oxidation parameters are 650°C thermal oxidation for 10 hours; the thicknesses of the thermal oxidation layers after TOCr treatment are 2.5 μm, 10.0 μm, 18.0 μm, and 28.0 μm, respectively.
10. A titanium alloy surface with a magnetron sputtering pre-deposition layer and a thermal oxidation layer. It is characterized in that The titanium alloy is prepared by the method for preparing a titanium alloy surface by magnetron sputtering pre-deposition layer followed by thermal oxidation layer as described in any one of claims 1 to 9.