Black film, preparation method thereof and optical device

By adopting magnetron sputtering deposition technology in black films, using the combination of composite absorption coating and anti-reflection films, the existing black films are easily scratched and corroded, and the effects of high absorption and low reflection are achieved. , expand its scope of application.

CN119040824APending Publication Date: 2024-11-29ZHEJIANG CRYSTAL OPTECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163190.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing black films are prone to scratches and corrosion due to the use of metal materials to make absorbent coatings, which limits their use in certain applications.

Method used

Using magnetron sputtering deposition method, a composite absorbing coating formed of at least two target materials is deposited on the substrate, and an anti-reflective film layer is plated thereon to form a black film of hierarchical structure, using the composite absorbing coating and reducing The combined characteristics of the reflective film layer improve the scratch resistance and corrosion resistance of the black film.

Benefits of technology

Through the combination of composite absorption coating and anti-reflective film, the black film obtains high absorption and low reflection light absorption effects, solving the problems of easy scratches and corrosion, and expanding its scope of application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040824A_ABST
    Figure CN119040824A_ABST
Patent Text Reader

Abstract

The invention discloses a black film, a preparation method thereof and an optical device, and relates to the technical field of optics, the method comprises the following steps: depositing a first composite absorbing coating on a substrate by using at least two target materials through magnetron sputtering; and depositing an antireflection film layer on the first composite absorbing coating. The black film, the preparation method of the black film and the optical device have the advantages of scratch resistance and corrosion resistance, the problem that in the prior art, due to the fact that an absorbing coating is made of metal materials, the prepared black film is prone to being scratched and corroded can be solved, and the application range of the black film is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of optical technology, and in particular to a black film and a preparation method thereof, and an optical device. Background Art

[0002] Black film, due to its extremely high light absorption rate, is widely used in optical sensors for aerospace telescopes, mobile phones, infrared cameras, security fields, medical fields, vehicles and mobile devices to reduce stray light, reduce background noise, improve precision and signal-to-noise ratio, and plays a very important role in improving image contrast and clarity.

[0003] In the prior art, black film generally includes a substrate, an absorption coating and an anti-reflection film layer arranged in sequence. Among them, the absorption coating is usually made of metal materials (such as titanium, chromium), although it can achieve a light absorption effect with a reflectivity of less than 0.5%, but due to the shortcomings of metal materials such as soft texture and poor chemical stability, the obtained black film has problems such as easy scratching and corrosion, which limits the use of black film in certain applications. Summary of the invention

[0004] The purpose of the present invention is to provide a black film and a preparation method thereof, and an optical device, which have the advantages of scratch resistance and corrosion resistance, can solve the problem of easy scratching and corrosion of the black film obtained in the prior art due to the use of metal materials to make the absorption coating, and expand the application scope of the black film.

[0005] The embodiment of the present invention is achieved as follows:

[0006] According to a first aspect of an embodiment of the present invention, a method for preparing a black film is provided, the method comprising:

[0007] depositing a first composite absorbent coating on the substrate by magnetron sputtering using at least two target materials;

[0008] An anti-reflection film layer is deposited on the first composite absorption coating.

[0009] As an practicable manner, the step of depositing the first composite absorption coating on the substrate by magnetron sputtering using at least two target materials includes:

[0010] placing a substrate and at least two target materials in a closed chamber;

[0011] Evacuating the sealed chamber to form a vacuum environment;

[0012] Simultaneously introducing working gas and reaction gas into the sealed chamber;

[0013] A sputtering voltage is provided, and the working gas and the reaction gas are ionized to form working ions and reaction ions under the action of the sputtering voltage. The working ions bombard at least two of the target materials, and the reaction ions combine with target particles in at least two of the target materials to deposit on the substrate to form a first composite absorption coating.

[0014] As an practicable manner, the target material includes a first target material and a second target material, the first target material is made of titanium, niobium, tantalum or zirconium, and the second target material is made of silicon or aluminum; or, the target material includes a first target material, a second target material and a third target material, the first target material is made of titanium, niobium, tantalum or zirconium, the second target material is made of silicon or aluminum, and the third target material is made of titanium, niobium, tantalum, zirconium, silicon or aluminum.

[0015] As an practicable manner, the substrate is made of optical glass, stainless steel, aluminum or plastic; and / or the working gas is argon, and the reaction gas is nitrogen or a nitrogen-oxygen mixed gas.

[0016] As an practicable manner, the thickness of the first composite absorption coating is between 100 and 5000 nm.

[0017] As an practicable manner, the anti-reflection film layer includes a plurality of first component units stacked in sequence, each of the first component units includes a first refractive index material layer and a second refractive index material layer stacked, and the refractive index of the first refractive index material layer is greater than the refractive index of the second refractive index material layer.

[0018] As an practicable manner, the material of the first refractive index material layer is oxide, nitride or oxynitride, and the material of the second refractive index material layer is silicon dioxide or a silicon-aluminum mixture.

[0019] As an practicable manner, the number of the first component units is 1 to 30, and the thickness of each of the first component units is between 1 and 600 nm.

[0020] As an practicable manner, the anti-reflection film layer also includes a second component unit, which is arranged between two adjacent first component units. The second component unit is a second composite absorption coating, and the second composite absorption coating includes reactive ions of reactive gas and target particles of at least two target materials.

[0021] As an practicable manner, the number of the second component units is 1 to 10, and the thickness of each of the second component units is between 1 and 300 nm.

[0022] According to a second aspect of the embodiments of the present invention, a black film is provided, which is prepared by the above-mentioned black film preparation method.

[0023] According to a third aspect of the embodiments of the present invention, an optical device is provided, comprising the above-mentioned black film.

[0024] The beneficial effects of the embodiments of the present invention include:

[0025] The preparation method of the black film comprises: depositing a first composite absorption coating on a substrate by magnetron sputtering using at least two target materials; and depositing an anti-reflection film layer on the first composite absorption coating. Compared with the prior art, in which a single type of metal material is first used to prepare an absorption coating with a single performance, and then an anti-reflection film layer is plated to finally prepare a black film, the method for preparing a black film provided in the present application first deposits a first composite absorption coating on a substrate using at least two target materials through a magnetron sputtering process, and then finally prepares a black film by plating an anti-reflection film layer on the first composite absorption coating. The prepared black film can present a hierarchical structure consisting of a substrate, a first composite absorption coating and an anti-reflection film layer stacked in sequence, so that the prepared black film has the physical and chemical properties of the materials used by at least two target materials through the first composite absorption coating, and at the same time, the prepared black film has a high absorption light absorption effect through the first composite absorption coating, and the prepared black film has a low reflection light absorption effect through the anti-reflection film layer, so that the prepared black film has the advantages of scratch resistance and corrosion resistance. Therefore, the problem that the prepared black film is easy to be scratched and corroded due to the absorption coating made of metal materials in the prior art can be solved, and the application scope of the black film is expanded. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0027] Figure 1 One of the flow charts of the method for preparing the black film provided in an embodiment of the present invention;

[0028] Figure 2 The second flowchart of the method for preparing the black film provided by the embodiment of the present invention;

[0029] Figure 3 A schematic diagram of the structure of an anti-reflection film layer provided in the first embodiment of the present invention;

[0030] Figure 4 A schematic diagram of the structure of a black film provided in the first embodiment of the present invention;

[0031] Figure 5A schematic diagram of the structure of the black film during measurement provided by the first embodiment of the present invention;

[0032] Figure 6 A reflection spectrum diagram of the black film provided by the first embodiment of the present invention;

[0033] Figure 7 A schematic structural diagram of an anti-reflection film layer provided in a second embodiment of the present invention;

[0034] Figure 8 A schematic diagram of the structure of a black film provided in a second embodiment of the present invention;

[0035] Fig. 9 A schematic structural diagram of an anti-reflection film layer provided in a third embodiment of the present invention;

[0036] Fig.10 A schematic structural diagram of a black film provided in the third embodiment of the present invention.

[0037] Icon: 100 - black film; 10 - substrate; 20 - first composite absorption coating; 30 - anti-reflection film layer; 31 - first component unit; 311 - first refractive index material layer; 312 - second refractive index material layer; 32 - second component unit; 40 - cover plate. DETAILED DESCRIPTION

[0038] The embodiments set forth below represent information necessary to enable those skilled in the art to practice the embodiments, and illustrate the best mode for practicing the embodiments. After reading the following description with reference to the accompanying drawings, those skilled in the art will understand the concepts of the present disclosure, and will recognize the applications of these concepts not specifically proposed herein. It should be understood that these concepts and applications are within the scope of the present disclosure and the appended claims.

[0039] It should be understood that although the terms first, second, etc. can be used to describe various elements in this article, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. For example, without departing from the scope of the present disclosure, the first element may be referred to as the second element, and similarly, the second element may be referred to as the first element. As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0040] It should be understood that when an element (such as a layer, region or substrate) is referred to as "on another element" or "extending onto another element", it can be directly on another element or directly extended onto another element, or there can also be an intervening element. On the contrary, when an element is referred to as "directly on another element" or "directly extending onto another element", there is no intervening element. Similarly, it should be understood that when an element (such as a layer, region or substrate) is referred to as "on another element" or "extending onto another element", it can be directly on another element or directly extended onto another element, or there can also be an intervening element. On the contrary, when an element is referred to as "directly on another element" or "extending directly onto another element", there is no intervening element. It should also be understood that when an element is referred to as "connected" or "coupled" to another element, it can be directly connected or coupled to another element, or there can be an intervening element. On the contrary, when an element is referred to as "directly connected" or "directly coupled" to another element, there is no intervening element.

[0041] Relative terms such as “below” or “above” or “upper” or “lower” or “horizontal” or “vertical” may be used herein to describe the relationship of one element, layer or region to another element, layer or region as shown in the figures.

[0042] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit the present disclosure. As used herein, unless the context clearly indicates otherwise, the singular forms "a", "an", and "the" are intended to include the plural forms as well. It should also be understood that when used herein, the term "comprising" indicates the presence of the features, integers, steps, operations, elements, and / or parts, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts, and / or groups of the above.

[0043] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood by those skilled in the art to which the present disclosure belongs. It should also be understood that the terms used herein should be interpreted as having the same meaning as they do in the context of this specification and the relevant art, and should not be interpreted in an idealized or overly formal sense, unless clearly defined in this article.

[0044] Please refer to Figures 1 to 10 The present application provides a black film 100 and a preparation method thereof, and an optical device, which have the advantages of scratch resistance and corrosion resistance, and can solve the problem that the black film produced in the prior art is easy to be scratched and corroded due to the use of metal materials to make the absorption coating, thereby expanding the application scope of the black film 100.

[0045] Specifically, Figure 1 , Figure 4 , Figure 8 and Fig.10 As shown, in a first aspect of an embodiment of the present application, a method for preparing a black film 100 is provided, the method comprising:

[0046] S110, depositing a first composite absorption coating 20 on the substrate 10 by magnetron sputtering using at least two target materials;

[0047] It should be noted that, first of all, Figure 4 , Figure 8 and Fig.10 As shown, a substrate 10 is provided, and the substrate 10 is used as a material basis for thin film deposition, wherein the surface of the substrate 10 needs to be dry and clean, so as to facilitate thin film deposition on the surface of the substrate 10 in subsequent steps; secondly, as Figure 1 , Figure 4 , Figure 8 and Fig.10 As shown, a first composite absorbing coating 20 is deposited on the substrate 10 (or one side of the substrate 10), wherein the first composite absorbing coating 20 is coated by a magnetron sputtering process, and in the above-mentioned magnetron sputtering process, at least two target materials are used for co-sputtering, so that the prepared first composite absorbing coating 20 has the physical and chemical properties of the materials used by the above-mentioned at least two target materials. Regarding the materials actually used for the at least two target materials, those skilled in the art should be able to make reasonable selections and designs according to actual conditions, and no specific restrictions are made here.

[0048] S210 , depositing an anti-reflection film layer 30 on the first composite absorption coating 20 .

[0049] It should be noted that, then, please continue to refer to Figure 1 , Figure 4 , Figure 8 and Fig.10After the first composite absorption coating 20 is deposited, a thin film is continuously deposited on the first composite absorption coating 20 (or the side of the first composite absorption coating 20 away from the substrate 10) to form an anti-reflection film layer 30, thereby preparing a black film 100. The prepared black film 100 includes a substrate 10, a first composite absorption coating 20 and an anti-reflection film layer 30 which are sequentially stacked, so that the prepared black film 100 has the physical and chemical properties of at least two materials used in the target material through the first composite absorption coating 20, and the prepared black film 100 has a high absorption light absorption effect through the first composite absorption coating 20, and the prepared black film 100 has a low reflection light absorption effect through the anti-reflection film layer 30. As for the actual process of coating the anti-reflection film layer 30, the coating technology commonly used in the industry and laboratories can be adopted, and those skilled in the art should be able to make reasonable selections and designs according to actual conditions, and no specific restrictions are made here. For example, the anti-reflection film layer 30 may be deposited on the first composite absorption coating 20 by physical vapor deposition, chemical vapor deposition or atomic layer deposition.

[0050] Compared with the prior art, in which a single type of metal material is first used to prepare an absorption coating with a single performance, and then an anti-reflection film layer 30 is plated to finally prepare the black film 100, the preparation method of the black film 100 provided in the present application first deposits a first composite absorption coating 20 on a substrate 10 by a magnetron sputtering process using at least two target materials, and then the anti-reflection film layer 30 is plated on the first composite absorption coating 20 to finally prepare the black film 100, so that the prepared black film 100 can present a hierarchical structure consisting of a substrate 10, a first composite absorption coating 20 and an anti-reflection film layer 30 stacked in sequence. The first composite absorption coating 20 is used to make the obtained black film 100 have the physical and chemical properties of at least two materials used in the target materials. At the same time, the first composite absorption coating 20 is used to make the obtained black film 100 have a high absorption light absorption effect. In addition, the anti-reflection film layer 30 is used to make the obtained black film 100 have a low reflection light absorption effect, so that the obtained black film 100 has the advantages of scratch resistance and corrosion resistance. Therefore, it can solve the problem of easy scratch and corrosion of the obtained black film due to the use of metal materials to make the absorption coating in the prior art, and expand the application scope of the black film 100.

[0051] like Figure 2 As shown, as an practicable manner, S110, depositing a first composite absorption coating 20 on a substrate 10 by magnetron sputtering using at least two target materials includes:

[0052] S111, placing a substrate 10 and at least two target materials in a sealed chamber;

[0053] S112, evacuating the sealed chamber to form a vacuum environment;

[0054] S113, introducing working gas and reaction gas into the sealed chamber simultaneously;

[0055] S114, providing a sputtering voltage, the working gas and the reaction gas are ionized under the action of the sputtering voltage to form working ions and reaction ions, the working ions bombard at least two target materials, the reaction ions combine with the target particles in the at least two target materials to deposit on the substrate 10 to form a first composite absorption coating 20.

[0056] It should be noted that in the actual coating process, the actual value of the sputtering voltage can be one or more, and those skilled in the art should be able to make reasonable selections and designs according to the actual situation, and no specific restrictions are made here. For example, when the sputtering voltages of the materials actually used by at least two target materials are close, at least two target materials can be co-sputtered simultaneously by one sputtering voltage; when the sputtering voltages of the materials actually used by at least two target materials are greatly different, at least two target materials can be co-sputtered separately or simultaneously by at least two sputtering voltages.

[0057] As an practicable manner, in some embodiments, the target material includes a first target material and a second target material, the first target material is made of titanium, niobium, tantalum or zirconium, and the second target material is made of silicon or aluminum; or, in other embodiments, the target material includes a first target material, a second target material and a third target material, the first target material is made of titanium, niobium, tantalum or zirconium, the second target material is made of silicon or aluminum, and the third target material is made of titanium, niobium, tantalum, zirconium, silicon or aluminum, so that the obtained first composite absorption coating 20 has the physical and chemical properties of the materials used by the three targets at the same time; or, in other embodiments, the target material includes a first target material, a second target material, a third target material and a fourth target material, the first target material is made of titanium, niobium, tantalum or zirconium, the second target material is made of silicon or aluminum, and the third and fourth target materials are made of titanium, niobium, tantalum, zirconium, silicon or aluminum, so that the obtained first composite absorption coating 20 has the physical and chemical properties of the materials used by the four targets at the same time, and so on.

[0058] As an practicable manner, the material of the substrate 10 is optical glass, stainless steel, aluminum or plastic (such as PET). As an practicable manner, the working gas is argon, the above-mentioned working ions are argon ions, and the reaction gas is nitrogen or a nitrogen-oxygen mixed gas. When the reaction gas is nitrogen, the above-mentioned reaction ions are nitrogen ions accordingly; when the reaction gas is a nitrogen-oxygen mixed gas, the above-mentioned reaction ions can be nitrogen ions, oxygen ions, or both nitrogen ions and oxygen ions. Regarding the actual selection of the reaction gas, those skilled in the art can make a reasonable selection and design according to the actual material of the target material, and no specific limitation is made here.

[0059] As an practicable manner, the thickness of the first composite absorbing coating 20 is between 100 and 5000 nm. Regarding the actual thickness of the first composite absorbing coating 20, those skilled in the art should be able to make reasonable selections and designs according to actual conditions, and no specific restrictions are made here. For example, the thickness of the first composite absorbing coating 20 is 100 nm, 500 nm, 1000 nm, 3000 nm or 5000 nm, etc.

[0060] like Figure 3 and Figure 4 As shown, as an implementable manner, the anti-reflection film layer 30 includes a plurality of first component units 31 stacked in sequence, each first component unit 31 includes a first refractive index material layer 311 and a second refractive index material layer 312 stacked, and the refractive index of the first refractive index material layer 311 is greater than the refractive index of the second refractive index material layer 312, so that the obtained anti-reflection film layer 30 has a low-reflection light absorption effect.

[0061] As an implementable manner, the material of the first refractive index material layer 311 is an oxide (such as titanium oxide, niobium oxide, tantalum oxide or zirconium oxide, etc.), a nitride (such as silicon nitride, etc.) or a nitride oxide (such as silicon oxynitride, etc.), and the material of the second refractive index material layer 312 is silicon dioxide or a silicon-aluminum mixture. Those skilled in the art should be able to make reasonable selections and designs based on actual conditions. It is only necessary that the refractive index of the first refractive index material layer 311 is greater than the refractive index of the second refractive index material layer 312. No specific restrictions are made here.

[0062] like Figure 3 and Figure 4 As shown, as an implementable manner, the number of first component units 31 is 1 to 30, for example, the number of first component units 31 is 1, 3, 5, 10, 20 or 30, etc., and the thickness of each first component unit 31 is between 1 and 600 nm, for example, the thickness of each first component unit 31 is 1 nm, 10 nm, 50 nm, 100 nm, 300 nm or 600 nm, etc. Those skilled in the art should be able to make reasonable selections and designs based on actual conditions, and no specific limitations are made here.

[0063] For example, Figure 5 and Figure 6 As shown, in this embodiment, the substrate 10 is selected as optical glass, the material of the first target is titanium, the power range is set between 3 and 10 kW, the material of the second target is silicon, the power range is set between 5 and 10 kW, and the reaction gas is nitrogen. In this way, TiN can be deposited on the glass substrate 10. x -SiN yThe first composite absorption coating 20. In the above magnetron sputtering process, by controlling the power ratio of the target material, various first composite absorption coatings 20 with different absorption characteristics can be prepared to meet different application scenarios. Then, the material of the first refractive index material layer 311 is selected as titanium oxide, and the material of the second refractive index material layer 312 is silicon dioxide. In this way, an anti-reflection film layer 30 formed by stacking a plurality of first component units 31 in sequence can be deposited on the first composite absorption coating 20, wherein each first component unit 31 is composed of titanium oxide and silicon dioxide, and finally a black film 100 is prepared.

[0064] like Figure 5 and Figure 6 As shown, when measuring the above-mentioned black film 100, it is necessary to first glue the black film 100 and the cover plate 40 (such as optical glass), and then measure the reflectivity. The measurement position is located at the interface between the cover plate 40 and the black film 100. At this time, the black film 100 exhibits a "glass|TiN x -SiN y (1000nm)|TiO2(45nm)|SiO2(26nm)|TiO2(15nm)|SiO2(68nm)|TiO2(8nm)|glass”. Figure 6 As shown, it can be found through measurement that in this embodiment, the average reflectivity of the black film 100 prepared in the 400-700nm band is lower than 0.05%. In other words, the absorption rate of the black film 100 provided in this embodiment in the 400-700nm band is higher than 99.9%, achieving an excellent low-reflection, high-absorption light absorption effect.

[0065] like Figures 7 to 10 As shown, in order to further improve the light absorption effect of the black film 100, as an practicable manner, the anti-reflection film layer 30 further includes a second component unit 32, and the second component unit 32 is arranged between two adjacent first component units 31. Figure 7 and Figure 8 As shown, in some embodiments, the second component units 32 can be stacked together to form a whole, such as Fig. 9 and Fig.10 As shown, in other embodiments, the second component units 32 may also be disposed at different positions.

[0066] The second component unit 32 is substantially a second composite absorption coating, which includes reactive ions of reactive gas and target particles of at least two target materials. The second composite absorption coating is similar to the first composite absorption coating 20, and is deposited by using at least two target materials through a magnetron sputtering process, but the specific location and film thickness are different. Therefore, the coating process of the second composite absorption coating and the actual materials of the at least two target materials can be reasonably selected and designed with reference to the first composite absorption coating 20, and no specific restrictions are made here.

[0067] As an practicable manner, the number of the second component units 32 is 1 to 10, for example, the number of the second component units 32 is 1, 3, 5, 7 or 10, etc., and the thickness of each second component unit 32 is between 1 and 300 nm, for example, the thickness of each second component unit 32 is 1 nm, 10 nm, 50 nm, 100 nm or 300 nm, etc. Those skilled in the art should be able to make reasonable selections and designs based on actual conditions, and no specific limitations are made here.

[0068] In a second aspect of the embodiment of the present application, a black film 100 is provided, and the black film 100 is prepared by the above-mentioned preparation method of the black film 100, and the black film 100 includes a substrate 10, a first composite absorption coating 20 and an anti-reflection film layer 30 which are stacked in sequence. The anti-reflection film layer 30 includes a plurality of first component units 31 which are stacked in sequence, and each first component unit 31 includes a first refractive index material layer 311 and a second refractive index material layer 312 which are stacked, and the refractive index of the first refractive index material layer 311 is greater than the refractive index of the second refractive index material layer 312; or, the anti-reflection film layer 30 also includes a second component unit 32, and the second component unit 32 is arranged between two adjacent first component units 31, and the second component unit 32 is a second composite absorption coating, and the second composite absorption coating includes reactive ions of reactive gas and target particles of at least two target materials.

[0069] It should be noted that the specific structure of the black film 100 provided in this embodiment is the same as the preparation method of the black film 100 in the previous text. Those skilled in the art can infer the specific structure of the black film 100 based on the description of the preparation method of the black film 100 in the previous text, and this application will not repeat the description. Since the black film 100 provided in this embodiment is prepared by the preparation method of the black film 100 described above, the black film 100 has the same beneficial effects as the preparation method of the black film 100 described above, and will not be repeated here.

[0070] According to a third aspect of the embodiments of the present application, an optical device is provided, and the optical device includes the above-mentioned black film 100. Since the structure and beneficial effects of the black film 100 have been described in detail in the above-mentioned embodiments, they will not be described in detail here.

[0071] The above description is only an optional embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

[0072] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. A method for preparing a black film, characterized in that: The method comprises: depositing a first composite absorbent coating on a substrate by magnetron sputtering using at least two target materials; An anti-reflection film layer is deposited on the first composite absorption coating.

2. The method for preparing the black film according to claim 1, characterized in that: The method of depositing a first composite absorbing coating on a substrate by magnetron sputtering using at least two target materials comprises: placing a substrate and at least two target materials in a closed chamber; Evacuating the sealed chamber to form a vacuum environment; Simultaneously introducing working gas and reaction gas into the sealed chamber; A sputtering voltage is provided, and the working gas and the reaction gas are ionized to form working ions and reaction ions under the action of the sputtering voltage. The working ions bombard at least two of the target materials, and the reaction ions combine with target particles in at least two of the target materials to deposit on the substrate to form a first composite absorption coating.

3. The method for preparing the black film according to claim 2, characterized in that: The target material includes a first target material and a second target material, the first target material is made of titanium, niobium, tantalum or zirconium, and the second target material is made of silicon or aluminum; or, the target material includes a first target material, a second target material and a third target material, the first target material is made of titanium, niobium, tantalum or zirconium, the second target material is made of silicon or aluminum, and the third target material is made of titanium, niobium, tantalum, zirconium, silicon or aluminum.

4. The method for preparing the black film according to claim 2, characterized in that: The substrate is made of optical glass, stainless steel, aluminum or plastic; and / or the working gas is argon, and the reaction gas is nitrogen or a nitrogen-oxygen mixed gas.

5. The method for preparing the black film according to claim 1, characterized in that: The thickness of the first composite absorption coating is between 100 and 5000 nm.

6. The method for preparing a black film according to claim 1, characterized in that: The anti-reflection film layer includes a plurality of first component units stacked in sequence, each of the first component units includes a first refractive index material layer and a second refractive index material layer stacked, and the refractive index of the first refractive index material layer is greater than the refractive index of the second refractive index material layer.

7. The method for preparing the black film according to claim 6, characterized in that: The material of the first refractive index material layer is oxide, nitride or oxynitride, and the material of the second refractive index material layer is silicon dioxide or a silicon-aluminum mixture.

8. The method for preparing a black film according to claim 6, characterized in that: The number of the first component units is 1 to 30, and the thickness of each of the first component units is between 1 and 600 nm.

9. The method for preparing a black film according to claim 6, characterized in that: The anti-reflection film layer also includes a second component unit, which is arranged between two adjacent first component units. The second component unit is a second composite absorption coating, which includes reactive ions of reactive gas and target particles of at least two target materials.

10. The method for preparing a black film according to claim 9, characterized in that: The number of the second component units is 1 to 10, and the thickness of each of the second component units is between 1 and 300 nm.

11. A black film, characterized in that: The black film is prepared by the method for preparing the black film according to any one of claims 1 to 10.

12. An optical device, characterized in that: Comprising the black film as claimed in claim 11.