Preparation method of anion-exchange membrane electrolytic cell catalytic electrode, and product and application of anion-exchange membrane electrolytic cell catalytic electrode

By forming a nickel-cobalt iron catalyst with nanocone-nano needle structure on the foam nickel-based material through electrodeposition and hydrothermal synthesis method, the problems of slow anode reaction kinetics and poor catalyst durability in the anion exchange membrane electrolysis technology are solved, and the problem of slow anode reaction kinetics and poor catalyst durability in the anion exchange membrane electrolysis technology is achieved. Improved catalytic performance with high efficiency and low cost.

CN119040932AActive Publication Date: 2024-11-29CHINA UNIV OF PETROLEUM (EAST CHINA)

Patent Information

Application Number
CN202411179759.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

In the existing anion exchange membrane electrolytic technology, the reaction kinetics of the four-electron transfer process of the anode oxygen evolution reaction is slow and requires high overpotentials. In addition, traditional precious metal-based catalysts are costly, scarce and have poor durability, and non-precious metal-based catalysts have low activity and poor durability. , difficult to meet practical application needs.

Method used

Using foam nickel as the base material, nickel, cobalt, and iron non-precious metal catalysts are grown on it through electrodeposition and hydrothermal synthesis to form a self-supported anode catalytic electrode with a multi-level structure of nanocone-nano needles, avoiding ionomers The use simplifies the process and improves the durability and active area of ​​the catalyst.

Benefits of technology

It achieves low-cost and efficient catalytic performance, improves the durability of the anode and the reaction mass transfer ability, reduces the cost of the electrode, and improves the electrocatalytic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040932A_ABST
    Figure CN119040932A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a catalytic electrode of an anion exchange membrane electrolytic cell as well as a product and application of the catalytic electrode. On one hand, a non-noble metal material is used, so that the cost is reduced, and the method is simple and easy to operate; and on the other hand, the catalyst is grown on the substrate material in situ, so that the use of an ionomer is avoided, the process is simplified, and the self-supporting catalytic electrode has more excellent durability. Besides, the formed nanocone-nanoneedle multistage microstructure provides a larger active area for the electrode material, the material is more hydrophilic and aerophobic, and mass transfer in the reaction process is promoted. The multi-metal component introduced into the material also adjusts the electronic structure of the material, so that the catalytic performance is favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalytic electrode preparation, and in particular relates to a preparation method of a catalytic electrode for an anion exchange membrane electrolyzer, a product thereof and an application thereof. Background Art

[0002] Anion exchange membrane water electrolysis (AEMWE) is an emerging water electrolysis technology that can operate in a weak alkaline solution or pure water environment. Its electrolyzer uses cheap structural components, which can greatly reduce the cost and has broad application prospects. However, the four-electron transfer process in its anodic oxygen evolution reaction (OER) leads to slow intrinsic reaction kinetics and requires a high overpotential, which limits the wide application of AEMWE. Therefore, it is necessary to design efficient catalysts to overcome the reaction energy barrier and catalyze the reaction quickly and efficiently.

[0003] Traditional noble metal-based catalysts (such as Pt / C and Ir / C electrocatalysts) show excellent OER performance in alkaline media, but high cost, scarcity and poor stability have become important factors limiting their large-scale commercial application. To this end, researchers have tried many non-noble metal-based materials as OER catalysts for AEMWE, but there are always problems of low activity and poor durability, which makes it difficult to meet the needs of practical applications.

[0004] Many existing powder catalysts usually require alkaline ionomers to adhere to the base material. However, the adhesion between the catalyst coated by the ionomer and the gas / liquid diffusion layer is weak. The catalyst is easily detached during the reaction, resulting in reduced durability. It also limits the transfer of electrons and has poor conductivity, resulting in limited catalytic effect of the catalyst.

[0005] Therefore, how to prepare efficient, stable and low-cost electrocatalysts is a technical problem to be solved. Summary of the invention

[0006] The purpose of this section is to summarize some aspects of embodiments of the present invention and to briefly introduce some preferred embodiments.

[0007] As one aspect of the present invention, the present invention provides a method for preparing a catalytic electrode for an anion exchange membrane electrolyzer, which comprises:

[0008] (1) preparing an electrolyte: adding nickel salt, boric acid and ammonium salt into water and dispersing them to obtain an electrolyte;

[0009] (2) using nickel foam as a working electrode, an Ag / AgCl electrode as a reference electrode, and a Pt sheet electrode as a counter electrode, placing the three electrodes in the electrolyte for electrochemical deposition, and washing and drying the product to obtain Ni / NF;

[0010] (3) Dispersing iron salt and cobalt salt in water, adding Ni / NF to soak, heating to react, washing, and drying to obtain Ni-CoFe2O4 / NF.

[0011] As a preferred embodiment of the method for preparing the catalytic electrode of the anion exchange membrane electrolyzer described in the present invention: in step (1), the nickel salt includes nickel chloride, the ammonium salt includes ammonium chloride, and the molar ratio of the nickel salt, boric acid and ammonium salt is 1:1 to 1.5:1 to 2.

[0012] As a preferred embodiment of the method for preparing the catalytic electrode of the anion exchange membrane electrolyzer described in the present invention: in step (1), the concentration of boric acid is 1 to 1.5 M; the molar ratio of the nickel salt, boric acid and ammonium salt is 0.025:0.03 mol:0.043; the dispersion in water includes heating to 55 to 60°C after ultrasonic dispersion and adjusting the pH to 4.

[0013] As a preferred embodiment of the method for preparing the catalytic electrode of the anion exchange membrane electrolyzer of the present invention: in step (2), the electrochemical deposition is carried out at 20 mA cm -2 Electrochemical deposition was carried out at a constant current for 8 to 10 minutes.

[0014] As a preferred embodiment of the method for preparing the catalytic electrode of the anion exchange membrane electrolyzer described in the present invention: in step (3), the iron salt is ferric chloride, and the cobalt salt is cobalt nitrate; the molar ratio of the iron salt to the cobalt salt is 1 to 1.5:1.

[0015] As a preferred embodiment of the method for preparing the catalytic electrode of the anion exchange membrane electrolyzer of the present invention: in step (3), the molar ratio of the iron salt to the cobalt salt is 0.27:0.22; and the concentration of the iron salt is 18-20 mM.

[0016] As a preferred embodiment of the method for preparing the catalytic electrode of the anion exchange membrane electrolyzer of the present invention: in step (3), the immersion time is 1 to 1.5 hours; and the heating reaction is carried out at 120° C. for 12 to 14 hours.

[0017] As a preferred embodiment of the method for preparing the catalytic electrode of the anion exchange membrane electrolyzer described in the present invention: in step (2), the nickel foam is pretreated, and the pretreatment step is: immersing the nickel foam in a hydrochloric acid solution to remove oxidized impurities on the surface, then rinsing with ethanol and deionized water, and drying.

[0018] Beneficial effects of the present invention: The present invention develops a self-supporting anode catalytic electrode with a nanocone-nanoneedle multi-level microstructure for anion exchange membrane water electrolysis. First, nickel foam is used as a base material, and non-precious metals such as iron, cobalt, and nickel are used as raw materials, and a catalyst is in situ grown on the base material by electrodeposition and hydrothermal synthesis. On the one hand, the use of non-precious metal materials reduces costs, and the method is simple and easy to operate; on the other hand, the in situ growth of the catalyst on the base material avoids the use of ionomers, simplifies the process, and the self-supporting catalytic electrode has better durability. In addition, the formed nanocone-nanoneedle multi-level microstructure provides a larger active area for the electrode material, makes the material more hydrophilic and gas-repellent, and promotes mass transfer during the reaction. The multi-metal components introduced into the material also adjust the electronic structure of the material, which is beneficial to the improvement of the catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required for describing the embodiment, wherein:

[0020] Figure 1 SEM images of electrode materials before and after growing catalyst on nickel foam substrate.

[0021] Figure 2 XRD patterns of Ni-CoFe2O4 / NF catalytic electrode and comparative samples NiFe2O4 / NF and NiCi2O4 / NF.

[0022] Figure 3 These are the XPS total spectra of Ni-CoFe2O4 / NF catalytic electrode and comparative samples NiFe2O4 / NF, NiCi2O4 / NF, Ni / NF, and Ni Foam, as well as the Fe 2p, Co 2p, and Ni 2p spectra.

[0023] Figure 4 This is a comparison of the water contact angles of Ni-CoFe2O4 / NF catalytic electrode, Ni / NF and Ni Foam.

[0024] Figure 5 The performance and morphology comparison of Ni / NF electrode materials synthesized after different electrodeposition times.

[0025] Figure 6 A comparison of the performance and morphology of Ni / NF electrode materials synthesized at different current densities.

[0026] Figure 7 The performance and morphology comparison of Ni-CoFe2O4 / NF synthesized hydrothermally at different temperatures.

[0027] Figure 8The performance and morphology comparison of Ni-CoFe2O4 / NF hydrothermally synthesized with different reaction times.

[0028] Fig. 9 It is a comparison chart of the OER performance of Ni-CoFe2O4 / NF catalytic electrode and comparative samples NiFe2O4 / NF, NiCo2O4 / NF, Ni / NF, and Ni Foam in a three-electrode system, including linear sweep voltammetry curve, Tafel slope, Cdl curve, and electrochemical impedance spectroscopy.

[0029] Fig.10 The Ni-CoFe2O4 / NF catalytic electrode was subjected to the three-electrode system at 100 mA cm -2 With 500mA cm -2 Stability test curve under constant current density.

[0030] Fig.11 The performances of anion exchange membrane electrolyzers assembled with Ni-CoFe2O4 / NF catalytic electrode and commercial catalyst RuO2 / NF as anode and Pt / C catalyst as cathode are compared, including polarization curves and electrochemical impedance spectroscopy.

[0031] Fig.12 This study was conducted to test the stability of an anion exchange membrane electrolyzer assembled with Ni-CoFe2O4 / NF catalytic electrode as the anode and Pt / C catalyst as the cathode. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.

[0033] Embodiment 1:

[0034] Preparation steps of nickel-cobalt-iron trimetallic self-supporting electrode (Ni-CoFe2O4 / NF) based on nickel foam substrate: 2 cm × 3 cm, 1 mm thick, 95% porosity, 110 PPI, and 280 g m -2 The nickel foam is at 3 mol L -1Ultrasonicate in HCl solution for 30 minutes to remove oxidized impurities on the surface, and then rinse alternately with ethanol and deionized water. When the nickel foam is rinsed to neutrality, transfer it to a 60℃ vacuum drying oven to dry for use. Add 0.025mol NiCl2·6H2O, 0.03molH38O3, and 0.043mol NH4CI in a beaker in sequence, and then add 30mL H2O to it, and ultrasonicate for 30 minutes to make it evenly dispersed. Preheat the ultrasonically dispersed solution in a 60℃ water bath, and when it becomes a completely transparent blue-green solution, add NaOH to adjust its pH to 4. Cut the nickel foam that has been pre-treated with HCl as mentioned above into small pieces of 1cm×2cm in size, and use an electrode clamp to clamp the nickel foam as the working electrode; the Ag / AgCl electrode is used as the reference electrode; and the Pt sheet electrode is used as the counter electrode. The three electrodes are placed in the prepared electrolyte and charged at 20mA cm -2 Electrochemical deposition was performed at a constant current of 8 min. The sample obtained after deposition was rinsed with ethanol and deionized water, and dried in an oven at 60 ° C for 30 min. The surface of the nickel foam turned black, and the sample was recorded as Ni / NF. 0.27mmolFeCl3·6H2O, 0.22mmolCo(NO3)2·4H2O and 15mLH2O were added to a beaker in sequence and ultrasonicated in a water bath for 30 min. The ultrasonically dispersed solution was transferred to a 50mL hydrothermal kettle, and the 0.98mmolNi / NF prepared above was placed in the hydrothermal kettle and allowed to soak for 1h. The hydrothermal kettle was placed in a blast oven and reacted at 120 ° C for 12h. The sample after reaction was taken out, and its surface was thoroughly cleaned with ethanol and deionized water. The cleaned sample was placed in a vacuum oven and dried at 90 ° C for 4h to obtain the sample: Ni-CoFe2O4 / NF.

[0035] Embodiment 2:

[0036] Preparation steps of nickel-cobalt-iron trimetallic self-supporting electrode for AEM electrolytic cell membrane electrode: 1cm×1cm nickel foam is placed in 3molL -1Ultrasonicate in HCl solution for 30 minutes to remove oxidized impurities on the surface, and then rinse alternately with ethanol and deionized water. When the nickel foam is rinsed to neutrality, transfer it to a 60°C vacuum drying oven and dry it for use. Add 5μL Nafion solution (Nafion117) and 4mg Pt / C catalyst (40%) to 995μL ethanol solution as a slurry; ultrasonicate the slurry in an ice bath (40kHz) for 20 minutes to evenly disperse the slurry. Use a pipette to take the slurry 100 times (10μL each time) and drop it onto the nickel foam pretreated with HCl. After drying under an infrared lamp, use it as the cathode material of the membrane electrode. The Ni-CoFe2O4 / NF synthesized in Example 1 was cut into a size of 1cm×1cm and used as the anode material of the membrane electrode. The Sustainion X37-50 membrane was cut into a size of 2cm×2cm and placed in 1molL -1 The membrane electrode was activated in KOH solution for 48 hours as an anion exchange membrane in the membrane electrode. The membrane electrode was assembled on the graphite bipolar plate through a PTFE gasket, and a torque of 5 N·m was used at all four corners to keep the force of the fixture uniform.

[0037] Comparative Example 1:

[0038] Preparation steps of HCl pre-treated nickel foam: 2cm×3cm nickel foam was placed in 3molL -1 The oxidized impurities on the surface were removed by ultrasonic treatment in HCl solution for 30 min, and then rinsed alternately with ethanol and deionized water. When the nickel foam was rinsed to neutrality, it was transferred to a 60°C vacuum drying oven and dried to obtain a sample, which was recorded as Ni Foam.

[0039] Comparative Example 2:

[0040] Preparation steps for electrochemical deposition of nickel metal on nickel foam: add 0.025molNiCl2·6H2O, 0.03mol H3BO3, 0.043mol NH4Cl in a beaker in sequence, then add 30mL H2O, and ultrasonicate for 30 minutes to disperse it evenly. Preheat the solution after ultrasonic dispersion in a 60℃ water bath, and when it becomes a completely transparent blue-green solution, add NaOH to adjust its pH to 4. Cut the nickel foam after HCl pretreatment into small pieces of 1cm×2cm, and use an electrode clamp to clamp the nickel foam as the working electrode; the Ag / AgCl electrode is used as the reference electrode; and the Pt sheet electrode is used as the counter electrode. The three electrodes are placed in the prepared electrolyte at 20mA cm -2 Electrochemical deposition was performed at a constant current of 80°C for 8 minutes. The sample obtained after deposition was rinsed with ethanol and deionized water, and dried in an oven at 60°C for 30 minutes. The surface of the nickel foam turned black, and the sample was recorded as Ni / NF.

[0041] Comparative Example 3:

[0042] The preparation steps of the sample obtained by reducing the synthesis time of Ni / NF are as follows: the electrolyte is prepared according to the steps in Comparative Example 2. The three electrodes are placed in the prepared electrolyte at 20 mA cm -2 Electrochemical deposition was performed at a constant current of 4 min (the rest of the steps were the same as those in Comparative Example 2). The sample obtained after deposition was rinsed with ethanol and deionized water, and dried in an oven at 60° C. for 30 min. The surface of the nickel foam turned black, and the sample was recorded as Ni / NF-1.

[0043] Comparative Example 4:

[0044] Preparation steps of the sample obtained by increasing the synthesis time of Ni / NF: prepare the electrolyte according to the steps in Comparative Example 2. Put the three electrodes into the prepared electrolyte at 20 mA cm -2 Electrochemical deposition was performed at a constant current of 1000 nm for 16 min (the rest of the steps were the same as those in Comparative Example 2). The sample obtained after deposition was rinsed with ethanol and deionized water, and dried in an oven at 60° C. for 30 min. The surface of the nickel foam turned black, and the sample was recorded as Ni / NF-2.

[0045] Comparative Example 5:

[0046] Preparation steps of the sample obtained by reducing the current density of Ni / NF synthesis: prepare the electrolyte according to the steps in Comparative Example 2. Put the three electrodes into the prepared electrolyte at 10 mA cm -2 Electrochemical deposition was performed at a constant current of 80°C for 8 minutes (the rest of the steps were the same as those in Comparative Example 2). The sample obtained after deposition was rinsed with ethanol and deionized water, and dried in an oven at 60°C for 30 minutes. The surface of the nickel foam turned black, and the sample was recorded as Ni / NF-3.

[0047] Comparative Example 6:

[0048] Preparation steps of the sample obtained by improving the current density of Ni / NF synthesis: prepare the electrolyte according to the steps in Comparative Example 2. Put the three electrodes into the prepared electrolyte at 40 mA cm -2 Electrochemical deposition was performed at a constant current of 80°C for 8 minutes (the rest of the steps were the same as those in Comparative Example 2). The sample obtained after deposition was rinsed with ethanol and deionized water, and dried in an oven at 60°C for 30 minutes. The surface of the nickel foam turned black, and the sample was recorded as Ni / NF-4.

[0049] Comparative Example 7:

[0050] Preparation steps of the sample obtained by lowering the hydrothermal synthesis temperature of Ni-CoFe2O4 / NF: Prepare the solution according to the steps in Example 1. Transfer the ultrasonically dispersed solution to a 50mL hydrothermal kettle, then put Ni / NF into the kettle and let it soak for 1h. Put the hydrothermal kettle into a blast oven and react at 100℃ for 12h (the rest of the steps are the same as Example 1), take out the reacted sample, thoroughly clean its surface with ethanol and deionized water, put the cleaned sample into a vacuum oven and dry it at 90℃ for 4h to obtain the sample: Ni-CoFe2O4 / NF-1.

[0051] Comparative Example 8:

[0052] Preparation steps of the sample obtained by increasing the hydrothermal synthesis temperature of Ni-CoFe2O4 / NF: Prepare the solution according to the steps in Example 1. Transfer the ultrasonically dispersed solution to a 50mL hydrothermal kettle, then put Ni / NF into the kettle and let it soak for 1h. Put the hydrothermal kettle into a blast oven and react at 160°C for 12h (the rest of the steps are the same as Example 1). Take out the reacted sample, clean its surface thoroughly with ethanol and deionized water, put the cleaned sample into a vacuum oven and dry it at 90°C for 4h to obtain the sample: Ni-CoFe2O4 / NF-2.

[0053] Comparative Example 9:

[0054] The steps for preparing the sample obtained by reducing the hydrothermal synthesis time of Ni-CoFe2O4 / NF are as follows: prepare the solution according to the steps in Example 1. Transfer the ultrasonically dispersed solution to a 50mL hydrothermal kettle, then put Ni / NF into the kettle and let it soak for 1h. Put the hydrothermal kettle into a blast oven and react at 160°C for 10h (the rest of the steps are the same as in Example 1). Take out the reacted sample, clean its surface thoroughly with ethanol and deionized water, put the cleaned sample into a vacuum oven and dry it at 90°C for 4h to obtain the sample: Ni-CoFe2O4 / NF-3.

[0055] Comparative Example 10:

[0056] Preparation steps of the sample obtained by increasing the hydrothermal synthesis time of Ni-CoFe2O4 / NF: Prepare the solution according to the steps in Example 1. Transfer the ultrasonically dispersed solution to a 50mL hydrothermal kettle, then put Ni / NF into the kettle and let it soak for 1h. Put the hydrothermal kettle into a blast oven and react at 120°C for 16h (the rest of the steps are the same as Example 1). Take out the reacted sample, clean its surface thoroughly with ethanol and deionized water, put the cleaned sample into a vacuum oven and dry it at 90°C for 4h to obtain the sample: Ni-CoFe2O4 / NF-4.

[0057] Comparative Example 11:

[0058] Preparation steps of nickel-cobalt bimetallic catalytic electrode material: Add 0.22mmolCo(NO3)2·4H2O and 15mL H2O in a beaker and ultrasonicate in a water bath for 30min. Transfer the ultrasonically dispersed solution to a 50mL hydrothermal kettle, then put Ni / NF into the kettle and let it soak for 1h. Put the hydrothermal kettle into a blast oven and react at 120℃ for 12h. Take out the reacted sample, clean its surface thoroughly with ethanol and deionized water, put the cleaned sample into a vacuum oven and dry it at 90℃ for 4h, and the obtained sample is recorded as: NiCi2O4 / NF.

[0059] Comparative Example 12:

[0060] Preparation steps of nickel-iron bimetallic catalytic electrode material: Add 0.27mmolFeCl3·6H2O and 15mL H2O in a beaker and ultrasonicate in a water bath for 30min. Transfer the ultrasonically dispersed solution to a 50mL hydrothermal kettle, then put Ni / NF into the kettle and let it soak for 1h. Put the hydrothermal kettle into a blast oven and react at 120℃ for 12h. Take out the reacted sample, clean its surface thoroughly with ethanol and deionized water, put the cleaned sample into a vacuum oven and dry it at 90℃ for 4h, and the obtained sample is recorded as: NiFe2O4 / NF.

[0061] Comparative Example 13:

[0062] The preparation steps of commercial RuO2 catalyst as anode for AEM electrolyzer membrane electrode are as follows: 1 cm × 1 cm nickel foam is heated in 3 mol L -1Ultrasonicate in HCl solution for 30 minutes to remove oxidized impurities on the surface, and then rinse with ethanol and deionized water alternately. When the nickel foam is rinsed to neutrality, transfer it to a 60℃ vacuum drying oven to dry for use. Add 5μL Nafion solution (Nafion117) and 4mg Pt / C catalyst (40%) to 995μL ethanol solution as slurry; ultrasonicate the slurry in an ice bath (40kHz) for 20 minutes to disperse the slurry evenly. Use a pipette to take the slurry 100 times (10μL each time) and drop it on the nickel foam pretreated with HCl, and use it as the cathode material of the membrane electrode after drying under an infrared lamp. Take the same size of nickel foam and perform HCl pretreatment according to the above method for use. Add 5μL Nafion solution (Nafion117) and 4mg RuO2 catalyst (>95wt%) to 995μL ethanol solution as slurry; ultrasonicate the slurry in an ice bath (40kHz) for 20 minutes to disperse the slurry evenly. Use a pipette to take the slurry 100 times (10 μL each time) and drop it onto the nickel foam pretreated with HCl. After drying under an infrared lamp, it is used as the anode material of the membrane electrode. Cut the SustainionX37-50 membrane into 2 cm × 2 cm size and put it into 1 mol L -1 The membrane electrode was activated in KOH solution for 48 hours as an anion exchange membrane in the membrane electrode. The membrane electrode was assembled on the graphite bipolar plate through a PTFE gasket, and a torque of 5 N·m was used at all four corners to keep the force of the fixture uniform.

[0063] Material Characterization: Figure 1 SEM images of the electrode material surface before and after the reaction (a) Comparative Example 1 (b) Comparative Example 2 (c) Example 1.

[0064] Nickel foam as a substrate material has a relatively smooth surface before the reaction. Figure 1 a. After electrochemical deposition, many cone-shaped structures are formed on the surface of nickel foam, and the material is recorded as Ni / NF. Figure 1 b, this structure has a smaller radius of curvature, which is beneficial to the hydrophilicity and gas repellency of the material, and promotes mass transfer; it has a larger active area than nickel foam Ni / NF. By further hydrothermal reaction of Ni / NF, a sample with a nanocone-nanonee multi-level structure was synthesized, denoted as Ni-CoFe2O4 / NF, see Figure 1 c. This structure has a smaller curvature radius than Ni / NF, providing more active sites for OER reactions and being more conducive to the removal of bubbles.

[0065] Figure 2 XRD test of electrode materials: (a) Example 1 and Comparative Example 2; (b) Comparative Example 11; (c) Comparative Example 12.

[0066] In order to explore the structural composition of the prepared electrode materials, we conducted corresponding XRD tests. Figure 2 In a, the peaks at 35.4°, 56.9° and 62.5° in the XRD spectrum of Example 1 correspond to the (311), (511) and (440) planes of CoFe2O4 (PDF#22-1086), respectively. The peaks at 44.5°, 51.8° and 76.3° in the XRD spectrum of Comparative Example 2 correspond to the (111), (200) and (220) planes of Ni (PDF#04-0850), respectively. The XRD spectrum of Example 1 also has corresponding peaks, so it can be determined that the sample composition of Example 1 is Ni-CoFe2O4. The XRD spectra of Comparative Examples 11 and 12 correspond well to the PDF cards of NiCo2O4 (PDF#02-1074) and NiFe2O4 (PDF#54-0964), respectively, see Figure 2 b and Figure 2 c. It can be determined that the sample compositions of Comparative Examples 11 and 12 are NiCo2O4 and NiFe2O4.

[0067] Figure 3 XPS test comparison of Example 1 and Comparative Examples 2, 11, and 12: (a) total spectrum; (b) Fe 2p spectrum; (c) Co 2p spectrum; and (d) Ni 2p spectrum.

[0068] In order to explore the elemental composition and element valence of the material, we conducted corresponding XPS tests. First, Figure 3 a is the XPS total spectrum of Example 1 and Comparative Examples 2, 11, and 12. From the total spectrum, it can be seen that Ni-CoFe2O4 / NF contains Ni, Co, Fe, O and other elements. In order to explore the regulation of the electronic structure by each element, we tested the spectra of each element and judged the role of different elements in regulating the electronic structure of the material based on the displacement of the element peaks in the spectra. By performing peak separation on the Fe 2p spectra of Ni-CoFe2O4 / NF and NiFe2O4 / NF, we can see Figure 3 b, it can be seen that the Fe 2p spectrum is fitted into a pair of identifiable peaks: the iron 2P3 / 2 peak at 713.6 eV and the Fe 2P1 / 2 peak at 725.4 eV. 3 / 2 peak and Fe2P at 724.8 eV 1 / 2 The peaks were deconvoluted to clearly reveal the Fe 3+ The presence of Co in the material Fe 3+The characteristic peak of Ni-CoFe2O4 / NF and NiCo2O4 / NF moves to the low binding energy direction, and the electron transfers from Co to Fe, indicating the electron-rich structure of Fe. The electron-rich Fe site enhances the OER activity. Figure 3 c, it can be seen that the Co 2p XPS spectrum can be deconvoluted into Co 3+ and Co 2+ Two peaks. It can be clearly seen from the figure that compared with NiCo2O4 / NF, the Co 2p3 / 2 in Ni-CoFe2O4 / NF is positively shifted. This further confirms that the electrons are transferred from Co to Fe. Finally, the Ni 2p spectra of Ni-CoFe2O4 / NF and Ni / NF were separated by peak processing. Figure 3 d, although Ni-CoFe2O4 / NF has similar Ni 2+ (854.8eV) and Ni 3+ (855.4eV) chemical state, due to the synergistic induction effect of Co and Fe, the Ni of Ni-CoFe2O4 / NF 3+ The peak has a negative shift of 0.2 eV compared to Ni / NF, which proves that electrons are also transferred to Ni. The incorporation of Co and Fe adjusts the electronic structure of the substrate Ni and promotes the electron transfer of the material.

[0069] Figure 4 Comparison of water contact angle test between Example 1 and Comparative Examples 1 and 2: (a) Comparative Example 1 (b) Comparative Example 2 (c) Example 1 1s before water contact (d) Example 1 1s after water contact.

[0070] To explore the relationship between material structure and hydrophilicity and hydrophobicity, we conducted a water contact angle test on the electrode material. First, the water contact angle of nickel foam was tested. Figure 4 a, its water contact angle is 106°, indicating that the nickel foam without any catalytic material is a hydrophobic structure. The water contact angle of the material Ni / NF obtained by electrochemical deposition of nickel foam is tested, see Figure 4 b, its water contact angle is 39°. Combined with the SEM test results, it shows that the conical structure electrochemically deposited on nickel foam changes the hydrophilicity of the material, and the material exhibits hydrophilic properties. The water contact angle test of Ni-CoFe2O4 / NF obtained by further hydrothermal reaction of Ni / NF found that the water droplet was absorbed by the material the moment it touched the material. Figure 4 c, d. Combined with the SEM test results, it is shown that the nanoneedle-like structure further grown on the Ni / NF nanocone structure has a smaller radius of curvature and is a more hydrophilic and gas-repellent structure. The electrode material is transformed into a super-hydrophilic material after having a nanocone-nanonee multi-level structure.

[0071] Figure 5 Comparison of the performance and morphology of Ni / NF synthesized with different electrodeposition times, (a) performance diagram (b) SEM morphology of comparative example 2 (c) SEM morphology of comparative example 3 (d) SEM morphology of comparative example 4.

[0072] To investigate the effect of electrodeposition time on the performance of synthesized Ni / NF electrode materials, we conducted a series of experiments at a fixed current density (20 mA cm -2 ) were used to prepare the electrode materials with different reaction times and the linear sweep voltammetry (LSV) curves were tested. The LSV curves of the electrode materials were tested at 1 mol L -1 The test was conducted in a KOH solution, with the synthesized electrode material as the working electrode, the platinum electrode as the counter electrode, the Hg / HgO electrode as the reference electrode, and the voltage set to 0-1V (compared to the reversible hydrogen electrode (RHE)). Overpotential is a key parameter in the LSV curve to judge the OER performance of the electrode material. It is the difference between the required potential and the theoretical potential when the reaction reaches a specific current density. The theoretical voltage of the water electrolysis reaction is 1.23V (vs. RHE), so η=E RHE -1.23V, E RHE is the actual electrode potential required. Generally, the overpotential of the catalyst under the same current density is compared on the LSV curve. The smaller the overpotential value, the better the catalytic performance of the catalyst. Figure 5 It can be seen from a that at a current density of 20 mA cm -2 When the deposition time is 8 min, the electrode material obtained has the smallest overpotential and the best OER performance. To explore the reasons why the samples obtained at different deposition times have different OER performance, we performed SEM characterization on the samples. When the deposition time is 4 min, there are only a few linear structures on the surface of the sample. Figure 5 c, failed to form a cone-like structure with the best OER performance, see Figure 5 b. When the electrodeposition time is further extended, cross-linking occurs on the surface of the material, thus destroying the conical structure of the material. Figure 5 d. The emergence of this cross-linked structure may be the reason for the decline in the performance of the electrode material.

[0073] Figure 6 Comparison of the performance and morphology of Ni / NF synthesized by electrodeposition at different current densities (a) Performance diagram (b) SEM morphology of comparative example 2 (c) SEM morphology of comparative example 5 (d) SEM morphology of comparative example 6.

[0074] In order to explore the effect of the current density used in the electrodeposition reaction on the performance of the synthesized Ni / NF electrode material, we conducted LSV curve tests on the electrode materials prepared with the optimal electrodeposition time (8 min) and different current densities. -2 The Ni / NF synthesized under the above conditions still has the best OER performance, see Figure 6 a. When the current density used in electrodeposition of electrode materials is reduced, the synthesized samples have only a small number of conical structures, and most of them are "stone-like" structures with a large radius of curvature, see Figure 6 c. This structure is not conducive to the mass transfer process of the catalytic electrode, which may be the reason for the decline in the performance of the electrode material. When the current density used in electrodeposition is increased, serious cross-linking occurs on the surface of the material, destroying the original cone structure. Figure 6 d, thus leading to the degradation of the catalytic electrode performance.

[0075] Figure 7 Comparison of the performance and morphology of Ni-CoFe2O4 / NF hydrothermally synthesized at different temperatures (a) Performance diagram (b) SEM morphology of Example 1 (c) SEM morphology of Comparative Example 7 (d) SEM morphology of Comparative Example 8.

[0076] In order to explore the effect of hydrothermal reaction temperature on the performance of synthesized Ni-CoFe2O4 / NF electrode materials, we conducted LSV curve tests on the synthesized materials under different temperature conditions with the same reaction time (12h). Figure 7 In a, Ni-CoFe2O4 / NF synthesized at 120℃ has the smallest overpotential, that is, the best OER performance. To explore the reason for this performance difference, we also performed SEM tests on several comparative examples to study the relationship between their structure and performance. When the material was synthesized at 100℃, compared with the sample synthesized at 120℃, Figure 7 b, The nanoneedles are sparsely distributed on the surface, which may result in a reduction in the number of reactive sites, see Figure 7 c. Increasing the reaction temperature destroyed the original cone structure. Figure 7 d, which also causes the loss of active area and thus reduces the OER performance of the electrode material.

[0077] Figure 8 Performance and morphology comparison of Ni-CoFe2O4 / NF hydrothermally synthesized after different reaction times (a) Performance diagram (b) SEM morphology of Example 1 (c) SEM morphology of Comparative Example 9 (d) SEM morphology of Comparative Example 10.

[0078] In order to explore the effect of hydrothermal reaction time on the performance of synthesized Ni-CoFe2O4 / NF electrode materials, we conducted LSV curve tests on the materials synthesized at different reaction times at the optimal reaction temperature (120°C). The results showed that the electrode material synthesized after a reaction time of 12 hours had the best OER performance. Through SEM testing to study the structure-activity relationship of the catalytic electrode, it was found that the material synthesized after 10 hours of hydrothermal reaction had a more sparse nanocone and nanoneedle structure than the material synthesized after 12 hours of synthesis time, as shown in Figure 2. Figure 8 b, c, the reduction of active sites leads to the decline of the OER performance of the material. The nanoneedles formed by the electrode material synthesized by 16h hydrothermal reaction are more slender, destroying the original nanocone structure. Figure 8 d, resulting in a decrease in material performance.

[0079] Fig. 9 Comparison of the three-electrode test performance of Example 1 and Comparative Examples 1, 2, 11, and 12: (a) LSV curve (b) Tafel slope (c) Cdl curve (d) electrochemical impedance spectroscopy diagram.

[0080] In order to explore the effect of the introduction of multi-metal components on the performance of electrode materials, we tested the LSV curve of the electrode material. Fig. 9 In a, Ni-CoFe2O4 / NF is heated to 100 mA cm -2 The overpotential is only 244mV, which is much lower than NiFe2O4 / NF (320mV), NiCo2O4 / NF (410mV) and Ni / NF (425mV) at the same current density. The overpotential of nickel foam at the same current density is as high as 500mV. It can be seen that Ni-CoFe2O4 / NF has the best OER catalytic performance. Compared with nickel foam, Ni / NF with a conical structure significantly reduces the OER overpotential, which shows that the conical structure has a promoting effect in increasing the electrochemical active area and mass transfer. Compared with NiCo2O4 / NF, NiFe2O4 / NF has better OER catalytic activity, which indicates that Fe is the main active site, and Ni-CoFe2O4 / NF has a lower overpotential than NiFe2O4 / NF, which shows that Co plays a role in adjusting the electronic structure and further improves the OER catalytic activity. The XPS test results also confirm this conclusion. Compared with nickel foam, Ni-CoFe2O4 / NF has a -2 The overpotential is significantly reduced at a current density of , indicating that the multi-level structure composed of the formed nanocones and nanoneedles also promotes OER.

[0081] The Tafel slope of the electrode material is calculated from the corresponding LSV curve. The Tafel slope is inversely proportional to the charge transfer coefficient. The stronger the charge transfer ability of the catalyst, the smaller the Tafel slope obtained. Fig. 9 In b, the Ni / NF sample with long nanocones electrodeposited on nickel foam has a higher conductivity than that of nickel foam (133 mVdec -1 ) has a smaller Tafel slope (89mV dec -1 ), and the Ni-CoFe2O4 / NF, NiFe2O4 / NF, and NiCi2O4 / NF obtained by hydrothermal synthesis of nanoneedle structures on Ni / NF samples have smaller Tafel slopes of 30 mV dec. -1 , 70mV dec -1 , 75mV dec -1 This indicates that both the nanocone structure on electrodeposition and the nanoneedle structure on hydrothermal treatment promote the OER electrochemical reaction kinetics of the catalyst, among which Ni-CoFe2O4 / NF has the smallest Tafel slope as the electrode material, indicating that it has the best electrochemical reaction kinetics, which can be attributed to the incorporation of Co and Fe metal components to regulate the electronic structure of the Ni substrate.

[0082] The electrochemically active area (ECSA) of the electrode material is positively correlated with the double layer capacitance (the slope of the Cdl curve). -1 ~100mV s -1 ) and the CV curve of the double layer current density (i c ) can be used to obtain the double-layer capacitance of the catalyst. Ni-CoFe2O4 / NF (20.81 mF cm -2 ) compared with Ni / NF (8.72 mF cm -2 ) and nickel foam (6.96mF cm -2 ) is much higher, see Fig. 9 c. The Cdl slope of Ni / NF is slightly higher than that of nickel foam, which indicates that the conical structure and needle-like structure synergistically provide a larger electrochemical active area. The larger the active area of ​​the electrode material, the greater the surface density of its active sites, which also represents a higher mass transfer rate and better overall catalytic activity.

[0083] At the same time, in order to further study the OER reaction kinetics of several catalytic electrode materials, their electrochemical impedance spectroscopy was collected at an overpotential of 300 mV. Fig. 9d. Ni-CoFe2O4 / NF has the smallest charge transfer resistance (0.5Ω), which is lower than NiFe2O4 / NF (0.8Ω), NiCo2O4 / NF (1.5Ω), Ni / NF (2Ω) and nickel foam (2.8Ω), indicating that Ni-CoFe2O4 / NF has faster charge transfer during OER, which can be attributed to the regulation of electronic structure by charge transfer between different elements and the acceleration of charge transfer by multi-level structure.

[0084] Fig.10 This is a stability test diagram of Example 1. To test the OER stability of Ni-CoFe2O4 / NF, chronopotentiometry was used to measure the OER stability of Ni-CoFe2O4 / NF at 1 mol L -1 In KOH solution, the current density was constant at 100 mA cm -2 and 500mA cm -2 The Ni-CoFe2O4 / NF catalytic electrode was tested under the conditions of 100 mA cm -2 At a current density of 1.7 V, the voltage was maintained constant for 100 h without decay; at 500 mA cm -2 The voltage was maintained at 1.6 V for 100 h without attenuation at a current density of Fig.10 This confirms that the Ni-CoFe2O4 / NF self-supporting catalytic electrode has good stability.

[0085] Fig.11 Performance comparison diagram of the AEM electrolytic cell of Example 2 and Comparative Example 13: (a) polarization curve and (b) electrochemical impedance diagram.

[0086] To explore the commercial application potential of Ni-CoFe2O4 / NF electrode materials, we conducted an AEM electrolytic cell performance test on the electrode material. The polarization curve of the electrolytic cell was obtained when the alkaline solution was introduced into the anode side at a flow rate of 8 ml min -1 , torque 5Nm -1 The test was conducted under the experimental conditions of 2000 ℃ and 80℃. We compared the performance of AEM electrolyzers with commercial Pt / C catalyst as cathode and Ni-CoFe2O4 / NF electrode material and RuO2 / NF commercial electrode material as anode. The polarization curves are shown in Fig.11 a. The electrolytic cell with Ni-CoFe2O4 / NF electrode material as the anode has excellent water electrolysis performance, reaching 1000mA cm at a voltage of 1.76V. -2 The industrial-grade current density is superior to that of commercial electrode material RuO2 / NF (1000 mA cm at 1.85 V). -2) electrolysis performance. To further compare the charge transfer resistance of the Ni-CoFe2O4 / NF electrode material and the RuO2 / NF commercial electrode material as anode, we tested their electrochemical impedance spectroscopy, see Fig.11 b. Compared with RuO2 / NF (1Ω), Ni-CoFe2O4 / NF electrode material has a smaller charge transfer resistance of 0.6Ω, indicating that Ni-CoFe2O4 / NF electrode material can also promote charge transfer in AEM electrolyzer, thereby improving the overall water electrolysis performance.

[0087] Fig.12 This is the stability test curve of the AEM electrolyzer in Example 2. To test the durability of the electrode material under high current density, we assembled an AEM electrolyzer with Ni-CoFe2O4 / NF electrode material as the anode and commercial Pt / C catalyst as the cathode for testing. The torque, temperature, and liquid flow rate conditions of the test were consistent with those of the polarization curve test. Fig.12 As shown, Ni-CoFe2O4 / NF||Pt / C at 1A cm -2 The voltage was stabilized at 1.9 V and the test lasted for 220 h without voltage decay, indicating that the Ni-CoFe2O4 / NF electrode material has good durability when operating at industrial-grade current density.

[0088] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a catalytic electrode for an anion exchange membrane electrolyzer, characterized in that: include, (1) preparing an electrolyte: adding nickel salt, boric acid and ammonium salt into water and dispersing them to obtain an electrolyte; (2) using nickel foam as a working electrode, an Ag / AgCl electrode as a reference electrode, and a Pt sheet electrode as a counter electrode, placing the three electrodes in the electrolyte for electrochemical deposition, and washing and drying the product to obtain Ni / NF; (3) Dispersing iron salt and cobalt salt in water, adding Ni / NF to soak, heating to react, washing, and drying to obtain Ni-CoFe2O4 / NF.

2. The method for preparing a catalytic electrode for an anion exchange membrane electrolyzer according to claim 1, characterized in that: In step (1), the nickel salt includes nickel chloride, the ammonium salt includes ammonium chloride, and the molar ratio of the nickel salt, boric acid, and ammonium salt is 1:1 to 1.5:1 to 2.

3. The method for preparing a catalytic electrode for an anion exchange membrane electrolyzer according to claim 1 or 2, characterized in that: In step (1), the concentration of boric acid is 1-1.5M; the molar ratio of the nickel salt, boric acid and ammonium salt is 0.025:0.03mol:0.043; and the dispersion in water includes heating to 55-60°C after ultrasonic dispersion and adjusting the pH to 4.

4. The method for preparing a catalytic electrode for an anion exchange membrane electrolyzer according to claim 1 or 2, characterized in that: In step (2), the electrochemical deposition is carried out at 20 mA cm -2 Electrochemical deposition was performed at a constant current of 8 to 10 min.

5. The method for preparing a catalytic electrode for an anion exchange membrane electrolyzer according to claim 1 or 2, characterized in that: In step (3), the iron salt is ferric chloride, and the cobalt salt is cobalt nitrate; the molar ratio of the iron salt to the cobalt salt is 1 to 1.5:

1.

6. The method for preparing a catalytic electrode for an anion exchange membrane electrolyzer according to claim 1 or 2, characterized in that: In step (3), the molar ratio of the iron salt to the cobalt salt is 0.27:0.22; and the concentration of the iron salt is 18-20 mM.

7. The method for preparing a catalytic electrode for an anion exchange membrane electrolyzer according to claim 1 or 2, characterized in that: In step (3), the soaking time is 1 to 1.5 hours; and the heating reaction is carried out at 120° C. for 12 to 14 hours.

8. The method for preparing a catalytic electrode for an anion exchange membrane electrolyzer according to claim 1 or 2, characterized in that: In step (2), the nickel foam is pretreated, and the pretreatment step is: immersing the nickel foam in a hydrochloric acid solution to remove oxidized impurities on the surface, then rinsing with ethanol and deionized water, and drying.

9. The anion exchange membrane electrolyzer catalytic electrode prepared by the preparation method according to claim 1.

10. Use of the anion exchange membrane electrolyzer catalytic electrode prepared by the preparation method according to claim 1 in preparing anion exchange membrane electrolyzer membrane electrode.

Citation Information

Patent Citations

  • Cobalt monoxide / cobalt ferrite nanosheet array structure catalyst rich in oxygen vacancies, preparation and application thereof

    CN113667993A

  • S-doped CoFe2O4 porous single crystal nanosheet assembled electrode material and preparation method thereof

    CN116623222A

Cited By

  • Sandwich-structure foam electrode for anion exchange membrane electrolyzed water as well as preparation method and application of sandwich-structure foam electrode

    CN121629434A