Preparation method and preparation device of defect-rich cyanation transition metal oxide material
Through the reaction of potassium ferrocyanide with transition metal nitrate and the use of sodium citrate, transition metal oxide materials with oxygen enriched vacancy and surface cyanation were prepared, and the lack of oxygen vacancy and surface cyanation materials in the prior art was solved. The problem has significantly improved the performance and selectivity of 2e-ORR electrocatalysts.
Patent Information
- Application Number
- CN202411085773.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-29
AI Technical Summary
The lack of methods for preparing oxygen vacant and surface cyanolated transition metal oxide materials in the prior art limits its performance improvement in 2e-ORR electrocatalysts.
Prussian blue analogue was prepared by reacting potassium ferricyanide with transition metal nitrate, using sodium citrate as complexing agent, and etching under an alkaline environment to obtain transition metal oxides with oxygen-rich vacanciation and surface cyanogenation. Material.
The excellent electrocatalytic performance and selectivity of the material are achieved, the charge transfer and reaction kinetics are enhanced, and the preparation process is simple and efficient.
Smart Images

Figure CN119040942A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energy materials, and in particular is a method and a device for preparing defect-rich cyanated transition metal oxide materials. Background Art
[0002] O at cathode 2 Electrochemical reduction reactions can selectively reduce oxygen to hydrogen peroxide at room temperature and pressure via the 2e-transfer pathway. This method has high hydrogen peroxide synthesis efficiency, as well as the advantages of economy, safety, environmental protection, and mildness. It can effectively solve the problems existing in the anthraquinone process for synthesizing hydrogen peroxide, and is considered to be an attractive and cost-effective strategy for hydrogen peroxide synthesis. More importantly, this method can be combined with cheap electricity (including solar or wind energy) in practical applications to produce hydrogen peroxide on a local, small-scale, on-demand basis. It can also produce hydrogen peroxide of different concentrations by controlling the reaction time, which not only reduces the cost problem during storage and transportation, but also solves the safety problem. Therefore, researchers are committed to developing efficient electrocatalysts to produce hydrogen peroxide.
[0003] Due to their surface effects and quantum size effects, transition metal catalysts exhibit electrochemical activity, stability and selectivity that are different from other catalysts, which greatly promotes the development of such catalysts in nanoscience and industrial applications. Due to the advantages of low cost, abundant earth reserves and good environmental compatibility of transition metal-based catalysts, they are widely used in the field of electrocatalytic synthesis of hydrogen peroxide. Although great progress has been made, the design concept and catalytic performance of 2e-ORR electrocatalysts still need further innovation. In order to solve these problems and further improve their 2e-ORR performance, vacancy engineering may be an effective method. Due to the reduced coordination number of surrounding atoms, the presence of vacancies in the lattice plane can change the surface chemical properties of transition metal-based materials, which is conducive to enhancing charge transfer and reaction kinetics. It is also possible to optimize OOH- adsorption and improve ORR performance by forming electron-withdrawing groups on the surface of the host material. However, there is no report in the patent literature on the simultaneous preparation of oxygen vacancies and surface cyanated transition metal oxides.
[0004] Therefore, how to provide a method and device for preparing defect-rich cyanated transition metal oxide materials is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide a method and a preparation device for defect-rich cyanated transition metal oxide materials, by reacting potassium ferrocyanide with transition metal nitrates, adding sodium citrate as a complexing agent, to obtain a transition metal-based Prussian blue analogue, and then etching in an etching component under an alkaline environment to obtain a transition metal oxide material with rich oxygen vacancies and surface cyanation, which can be used as an electrocatalyst for two-electron electrocatalytic oxygen reduction and can exhibit excellent catalytic activity and selectivity.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows: a method and a device for preparing defect-rich cyanated transition metal oxide materials, wherein the method for preparing the transition metal oxide material comprises the following steps:
[0007] Step 1, preparing a solution: dissolving substance A and substance B in deionized water to obtain solution A and solution B respectively;
[0008] Step 2, preparing a Prussian blue analogue: stirring and mixing solution A and sodium citrate dihydrate, adding solution B during stirring until a precipitate is precipitated, and the stirring time is 24 hours, and the stirred solution is centrifuged and washed 3-10 times with deionized water and anhydrous ethanol, and then the precipitate is filtered and dried to obtain a Prussian blue analogue;
[0009] Step three, prepare a transition metal oxide material rich in oxygen vacancies and surface cyanation: add the obtained Prussian blue analogue to an etching component, add an alkaline solution to the etching component, and perform etching for 5-10 minutes, then wash the etched Prussian blue analogue with deionized water and anhydrous ethanol for 3-10 times, and then dry the washed Prussian blue analogue to obtain a transition metal oxide material rich in oxygen vacancies and surface cyanation.
[0010] The following principles and beneficial effects are achieved by adopting the above scheme:
[0011] Basic principle: Potassium ferrocyanide is reacted with transition metal nitrates and sodium citrate is added as a complexing agent to obtain a transition metal-based Prussian blue analogue, which is then etched in an alkaline environment to obtain a transition metal oxide material with abundant oxygen vacancies and surface cyanation.
[0012] Beneficial effects: 1. The present invention uses Prussian blue analogs as precursors, which have rich defects and cyano structures and are good raw materials for preparing transition metal oxide materials rich in oxygen vacancies and surface cyanation.
[0013] 2. The transition metal oxide material with rich oxygen vacancies and surface cyanation prepared by the present invention is suitable for use as a 2e-ORR electrocatalyst. The electrochemical performance test of this electrocatalyst material shows excellent electrocatalytic performance in RRDE.
[0014] 3. Oxygen vacancies and surface cyanation The oxygen vacancies and surface cyanide functional groups of transition metal oxides can change the surface chemical properties of transition metal-based catalysts, which is beneficial to enhance charge transfer and reaction kinetics.
[0015] 4. The preparation method of the transition metal oxide material of the present invention is efficient and easy to implement, and the operation steps are simple, and only three steps are required to complete the process: solution preparation, precipitation and etching.
[0016] Further, in step 1, substance A includes Fe(NO 3 ) 2 、Fe(NO 3 ) 3 、Co(NO 3 ) 2 ,Ni(NO 3 ) 2 、Cu(NO 3 ) 2 、Zn(NO 3 ) 2 、Mn(NO 3 ) 2 、FeCl 2 、FeCl 3 、CoCl 2 、NiCl 2 , CuCl 2 、ZnCl 2 and MnCl 2 One or more of; Substance B includes K 3 [Fe(CN) 6 ], K 4 [Fe(CN) 6 ] and K 3 [Co(CN)6] or more.
[0017] Beneficial effects: Substance A contains a variety of transition metal elements (such as Fe, Co, Ni, Cu, Zn, Mn), which makes it possible to flexibly select and adjust the type and proportion of transition metals, thereby preparing transition metal oxide materials with different electronic structures and catalytic properties; different transition metal elements have different redox characteristics and catalytic activities. By mixing and using a variety of transition metals, the catalytic performance of the material can be synergistically enhanced, and its activity and selectivity in specific reactions (such as oxygen reduction reactions) can be improved; precursors such as transition metal nitrates can form abundant oxygen vacancies during subsequent reactions and etching processes. These oxygen vacancies, as active centers of catalytic reactions, have an important influence on the catalytic performance of the material. By adjusting the type and proportion of transition metals in substance A, the concentration and distribution of oxygen vacancies in the final product can be indirectly regulated; the Prussian blue analogues generated by the reaction of substance A with substance B (such as potassium ferrocyanide) have stable cyano functional groups. These cyano functional groups can be partially retained in the final product during the subsequent etching process, providing additional catalytic activity and stability for the material.
[0018] Furthermore, in step 1, the concentration of solution A is 37.5 mmol / L, and the concentration of solution B is 12.5 mmol / L.
[0019] Beneficial effect: The relatively high concentration of the transition metal salt solution A enables the reaction to proceed fully, which is beneficial for obtaining the Prussian blue analogue.
[0020] Furthermore, in step 2, the mass ratio of sodium citrate dihydrate to solution A is 3.3 g:250 mL, and the volume ratio of solution A to solution B is 1:1.
[0021] Beneficial effects: Sodium citrate dihydrate, as an additive in the reaction system, helps the reaction between transition metal ions and cyanide ions to proceed smoothly. The appropriate mass ratio can ensure that sodium citrate dihydrate fully plays its role in the reaction and promotes the formation of Prussian blue analogs.
[0022] Furthermore, in step 2, the stirring speed is 200 to 1000 r / min; the addition rate of solution B is V / 500 to V / 100 per minute; the drying treatment is one of vacuum drying treatment and freeze drying treatment, the temperature of the vacuum drying treatment is 60 to 100°C, the temperature of the freeze drying treatment is -35 to -50°C, and the drying treatment time is 10 to 24 hours.
[0023] Beneficial effects: Stirring can make the reactants fully contact each other, and by controlling the addition rate of solution B, the reaction process can be controlled to proceed slowly and gently, thereby obtaining a nanocubic structured Prussian blue analogue, and drying treatment can prevent the Prussian blue analogue from being further oxidized by long-term contact with air.
[0024] Furthermore, in step 3, the mass of the Prussian blue analogue is 750 mg, and the alkaline solution is 50 mL of 0.1 mol / L KOH.
[0025] Beneficial effect: By reacting a Prussian blue analogue with KOH, the corresponding transition metal oxide can be obtained, and the defect sites and cyano functional groups of the Prussian blue analogue can also be inherited.
[0026] Furthermore, in step three, the etching component includes a solution tank, the bottom of which is fixedly connected to and communicated with a nano bubble making machine, and a reactor component for etching the Lushi blue analog is arranged in the solution tank.
[0027] Beneficial effect: When the nanobubbles come into contact with the Prussian blue analogue during the rising process, their tail vortices will carry the Prussian blue analogue particles with them to rise together. This carrying effect helps the Prussian blue analogue particles to disperse and mix with KOH in the etching reaction system, so that the Prussian blue analogue particles and KOH particles can contact more fully, thereby further improving the purity of the obtained transition metal oxide material.
[0028] Furthermore, the reactor assembly includes a reaction container, a material taking port is opened on the side wall of the reaction container, a material taking door is hinged on the material taking port, a first nano filter plate is vertically slidably engaged with the inner wall of the reaction container, and a vibration extrusion assembly for extruding and vibrating the Lushi blue analog is provided on the top of the first nano filter plate.
[0029] Beneficial effects: The vibration extrusion component can make the Prussian blue analogue at the edge of the reaction container gradually move toward the middle and fully contact with the nanobubbles. At the same time, the vibration effect it produces further makes the Prussian blue analogue and KOH contact more fully.
[0030] Furthermore, the vibration extrusion assembly includes a sliding rod, one end of the sliding rod is fixedly connected to the top of the first nano filter plate, the end of the sliding rod away from the first nano filter plate is fixedly connected to a spring, the end of the spring away from the sliding rod is fixedly connected to the top cover, the inner wall of the top cover is symmetrically and fixedly connected with a triangular slider, and the triangular slider is set in reverse; an inclined groove is opened on the sliding rod, and a Z-shaped slider is slidably matched in the inclined groove, and both ends of the Z-shaped slider are slidably matched with adjacent triangular sliders, and the outer wall of the top cover is slidably matched with a base, and the outer wall of the base is fixedly connected with a second bracket, and the second bracket is fixedly connected to the inner wall of the reaction container at one end away from the base, and the inner bottom wall of the base is fixedly connected with a sliding cylinder, the sliding cylinder and the base are connected, the sliding rod passes through the sliding cylinder and vertically slides with the inner wall of the sliding cylinder, and a sliding groove is opened on the sliding cylinder, and the Z-shaped slider and the sliding groove are both vertically slidably matched; the inner wall of the reaction container is vertically slidably matched with a second nano filter plate, and a plurality of support rods are fixedly connected to the bottom of the second nano filter plate, and the bottoms of the support rods are fixedly connected to the top of the second nano filter plate.
[0031] Beneficial effects: the sliding rod and the top cover will drive the first nano filter plate to move downward, at which time the first nano filter plate will slide downward and the second nano filter plate will slide upward to restore to the initial position, and due to the intermittent blowing of nano bubbles and the continuous addition of Prussian blue analogs, the up and down sliding movement of the first nano filter plate and the second nano filter plate will be repeated, so that the first nano filter plate and the second nano filter plate produce a vibration effect on the internal Prussian blue analogs, and further make the Prussian blue analogs and KOH contact more fully; the first nano filter plate and the second nano filter plate will bring the Prussian blue analogs scattered in various corners together to prevent the Prussian blue analogs in some corners from reacting incompletely, and the nano bubble making machine is set to blow bubbles after the first nano filter plate and the second nano filter plate are brought together, which can greatly change the position of the Prussian blue analogs in the reaction container and improve the reaction effect.
[0032] Furthermore, a first bracket is fixedly connected to the inner wall of the solution tank, and a funnel is fixedly connected to one end of the first bracket away from the inner wall of the solution tank. The bottom of the funnel penetrates the second nano filter plate and extends to above the top cover. The bottom of the funnel and the part penetrating the second nano filter plate are vertically slidably matched, and the part where the bottom of the reaction container and the nano bubble making machine are connected is connected with a one-way valve.
[0033] Beneficial effect: The one-way valve is provided at this position to prevent KOH in the solution tank from flowing back into the nano bubble making machine and causing damage to the nano bubble making machine during the etching process. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a SEM image of the transition metal oxide material with oxygen-rich vacancies and surface cyanation in an embodiment of the present invention.
[0035] Figure 2 This is a TEM image of a transition metal oxide material with oxygen-rich vacancies and surface cyanation in an embodiment of the present invention.
[0036] Figure 3 This is a graph showing the XRD characterization results of the transition metal oxide material with oxygen vacancies and surface cyanation in an embodiment of the present invention.
[0037] Figure 4 This is a graph showing the XPS characterization results of the transition metal oxide material with oxygen-rich vacancies and surface cyanation in an embodiment of the present invention.
[0038] Figure 5 This is a graph showing the ERP characterization results of the transition metal oxide material with oxygen vacancies and surface cyanation in an embodiment of the present invention.
[0039] Figure 6 This is a graph showing the FT-IR characterization results of the transition metal oxide material with oxygen-rich vacancies and surface cyanation in an embodiment of the present invention.
[0040] Figure 7 The ORR energy of the catalyst in the electrochemical test results of Example 1 of the present invention and the simultaneous H 2 O 2 Comparison graph of detection current density.
[0041] Figure 8 is the H in the electrochemical test results in Example 1 of the present invention 2 O 2 Selective graph.
[0042] Fig. 9 This is a diagram of the number of transferred electrons in the electrochemical test results in Example 1 of the present invention.
[0043] Fig.10 This is the EIS impedance diagram of the electrochemical test results in Example 1 of the present invention.
[0044] Fig.11 The ORR performance of the catalyst in the electrochemical test results of Example 2 of the present invention and the H 2 O 2 Comparison graph of detection current density.
[0045] Fig.12 is the H in the electrochemical test results in Example 2 of the present invention 2 O 2 Selective graph.
[0046] Fig.13 This is a diagram of the number of transferred electrons in the electrochemical test results in Example 2 of the present invention.
[0047] Fig.14 This is the EIS impedance diagram of the electrochemical test results in Example 2 of the present invention.
[0048] Fig.15 It is an axonometric view of the etching component in an embodiment of the present invention.
[0049] Fig.16 It is a front cross-sectional view of the etching component in the embodiment of the present invention.
[0050] Fig.17 It is a front cross-sectional view of the vibration extrusion assembly in an embodiment of the present invention.
[0051] The figure numbers in the drawings of the specification include: 1, solution tank; 2, nano bubble making machine; 3, reaction container; 4, material taking port; 5, material taking door; 6, first nano filter plate; 7, slide rod; 8, spring; 9, top cover; 10, triangular slider; 11, inclined groove; 12, Z-shaped slider; 13, base; 14, slide cylinder; 15, slide groove; 16, support rod; 17, second nano filter plate; 18, first bracket; 19, funnel; 20, one-way valve. DETAILED DESCRIPTION
[0052] The following is further described in detail through specific implementation methods:
[0053] Embodiment 1:
[0054] Example 1 is basically as Figure 1-Figure 10 As shown:
[0055] A method for preparing a defect-rich cyanated transition metal oxide material comprises the following steps:
[0056] Step 1: Prepare the solution: slowly add 3.3 g of sodium citrate dihydrate into 250 mL of 37.5 mmol / L Zn(NO 3 ) 2 solution to obtain a mixed solution.
[0057] Step 2, prepare a Prussian blue analogue: add 250 mL of a 12.5 mmol / L K3[Fe(CN)6] solution at a rate of 1 mL / min at a stirring speed of 800 r / min. After stirring for 24 hours, the stirred solution is centrifuged until a precipitate is precipitated from the solution. The precipitate is filtered and washed with deionized water and anhydrous ethanol for 6 times until the filtrate is colorless. The precipitate is then freeze-dried for 12 hours to obtain a yellow-green Prussian blue analogue.
[0058] Step three, prepare a transition metal oxide material rich in oxygen vacancies and surface cyanation: weigh 750 mg of a Prussian blue analogue, add it to an etching component, then add 50 mL of 0.1 mol / L KOH, etch the Prussian blue analogue in the etching component, take out the etched Prussian blue analogue after 10 minutes, wash the etched Prussian blue analogue with deionized water and anhydrous ethanol for 6 times until the filtrate is colorless, and then freeze-dry the washed Prussian blue analogue for 12 hours to obtain a transition metal oxide material rich in oxygen vacancies and surface cyanation.
[0059] In this embodiment 1, the transition metal oxide material rich in oxygen vacancies and surface cyanation has abundant oxygen vacancies and surface cyano functional groups; the transition metal oxide material rich in oxygen vacancies and surface cyanation can use EPR characterization technology to determine whether oxygen vacancies exist, and the concentration of oxygen vacancies can be quantitatively obtained. The cyano functional groups on the surface can be confirmed by XPS and FT-IR characterization technology.
[0060] The oxygen-rich vacancies and surface cyanated transition metal oxide materials obtained in Example 1 are tested as follows:
[0061] The SEM image of the transition metal oxide material with oxygen-rich vacancies and surface cyanation prepared in Example 1 is as follows: Figure 1 As shown in the TEM image Figure 2 As shown in the figure, it can be seen that this transition metal oxide with oxygen vacancies and surface cyanation is a nano-scale particle with a porous structure similar to melon seeds.
[0062] The XRD characterization results of the transition metal oxide material with oxygen vacancies and surface cyanation prepared in Example 1 are as follows: Figure 3 As shown in the figure, it can be seen that the material is pure zinc oxide, which means that the corresponding metal oxide is obtained after etching in an alkaline environment.
[0063] In order to determine the vacancy content and cyanide functional groups of the transition metal oxide materials with oxygen vacancies and surface cyanation, the materials were characterized by XPS, EPR and FT-IR. Figure 4 As shown in the figure, the peaks belonging to cyanide at 285.50eV and 399.10eV can be seen in the fine spectrum of C1s and N1s, indicating that cyanide exists on the surface of the material. The peak belonging to oxygen defect at 531.56eV can be seen in the fine spectrum of O1s, indicating that there may be a large number of oxygen defects in the material. The EPR characterization results are shown in the figure. Figure 5 As shown in Figure 2, the oxygen vacancy signal at g = 2.004 can be seen, and the oxygen vacancy concentration is 8.5×10 14 spins / g. FT-IR characterization results are shown in Figure 6 As shown, at 2100cm -1 The stretching vibration peak of cyano group appears at , indicating that the material surface contains cyano group, which is consistent with the XPS results.
[0064] The electrochemical performance test of the transition metal oxide material with oxygen-rich vacancies and surface cyanation obtained in Example 1 is as follows:
[0065] The prepared oxygen-rich vacancies and the transition metal oxide material with surface cyanation were used as electrocatalysts. 5 mg of electrocatalyst, 950 μL of anhydrous ethanol, and 50 μL of 5% Nafion solution were mixed and ultrasonicated for 30 min to obtain a uniformly dispersed catalyst ink. 2 The experiment was carried out in saturated 0.1 mol / L KOH.
[0066] The workstation used was a CHI760E electrochemical workstation (Shanghai Chenhua). First, a rotating ring disk electrode (RRDE, glassy carbon (GC) disk, and Pt ring) and a three-electrode system (graphite rod as counter electrode, Hg / HgO as reference electrode) were used. The potential was converted to the reversible hydrogen electrode (RHE) scale by calibration using the following equation: E (vs. RHE) = E (vs. Hg / HgO) + 0.059 × pH + 0.098 V (all potentials in the present invention are based on the RHE scale), and the current density was converted to a geometric surface area. In order to accurately measure H 2 O 2 Selectivity: RRDE was thoroughly cleaned before each experiment. RRDE was polished with 1 μM alumina aqueous suspension for 10 min and sonicated in deionized water for 20 s. Catalyst-coated RRDE (disc area: 0.2475 cm) was prepared by spin coating (100 rpm). 2 , Ring area: 0.1866cm 2 ), 5 μL of catalyst ink was dropped on the GC disk and dried at room temperature before use. -1 Twenty cyclic voltammetry (CV) cycles were performed to obtain a stable CV response. Then, the Pt ring was charged between 0 and 1.2 V at 100 mV·s -1 Electrochemical scans were performed for 20 cycles. Electrochemical impedance spectroscopy (EIS) was performed at 0.865 V from 100 kHz to 0.1 Hz. 2 O 2 The selectivity was measured by linear sweep voltammetry (LSV) at a rotation speed of 1600 rpm and a scan rate of 20 mV·s -1 , from 0 to 1.0VO 2 Saturated 0.1 mol / L KOH. During the LSV process, the Pt ring potential was maintained at 1.2 V.
[0067] The electrochemical test results are as follows Figure 7-10 As shown:
[0068] Figure 7 The ORR performance of the catalyst (bottom) and the simultaneous H 2 O 2 Comparison of detection current density (top). The results show that it has a relatively high starting potential of 0.67V and a current density of 2.3mA / cm 2 The ORR current density is 1.0mA / cm 2 The ring current density indicates that there is a large amount of H 2 O 2 generate.
[0069] Figure 8H 2 O 2 Selectivity plots show that the catalyst is able to maintain an average of 95% H 2 O 2 Selective.
[0070] Fig. 9 The results show that the number of transferred electrons of the catalyst is close to 2, and the ORR pathway is a two-electron pathway to generate H 2 O 2 .
[0071] Fig.10 The EIS impedance diagram shows that the catalyst has a charge transfer resistance of 35Ω, and the high slope in the low-frequency region indicates that its mass diffusion rate is faster.
[0072] Embodiment 2:
[0073] Example 2 is basically the same Figure 11-Figure 14 As shown:
[0074] The difference from the above embodiment is that the transition metal oxide material with oxygen vacancies and surface cyanation can be directly used as an electrocatalyst in the 2e-ORR reaction process, and the ink mixed with anhydrous ethanol and 5% Nafion solution is used as an electrocatalyst for electrocatalytic oxygen reduction to synthesize hydrogen peroxide in a three-electrode system.
[0075] A method for preparing a defect-rich cyanated transition metal oxide material in Example 2 comprises the following steps:
[0076] Step 1: Prepare the solution: slowly add 3.3 g of sodium citrate dihydrate into 250 mL of 37.5 mmol / L Cu(NO 3 ) 2 solution to obtain a mixed solution.
[0077] Step 2, prepare a Prussian blue analogue: add 250 mL of a 12.5 mmol / L K3[Fe(CN)6] solution at a rate of 3 mL / min at a stirring speed of 1000 r / min. After stirring for 24 hours, the stirred solution is centrifuged until a precipitate is precipitated from the solution. The precipitate is filtered and washed with deionized water and anhydrous ethanol for 6 times until the filtrate is colorless. The precipitate is then freeze-dried for 12 hours to obtain a yellow-green Prussian blue analogue.
[0078] Step three, prepare a transition metal oxide material rich in oxygen vacancies and surface cyanation: weigh 750 mg of a Prussian blue analogue, add it to an etching component, etch the Prussian blue analogue in the etching component, then add 50 mL of 0.1 mol / L KOH, take out the etched Prussian blue analogue after 10 minutes, wash the etched Prussian blue analogue with deionized water and anhydrous ethanol for 6 times until the filtrate is colorless, and then freeze-dry the washed Prussian blue analogue for 12 hours to obtain a transition metal oxide material rich in oxygen vacancies and surface cyanation.
[0079] The transition metal oxide material with oxygen vacancies and surface cyanation obtained in Example 2 was used as an electrocatalyst. 5 mg of the electrocatalyst, 950 μL of anhydrous ethanol, and 50 μL of 5% Nafion solution were mixed and ultrasonicated for 30 min to obtain a uniformly dispersed catalyst ink. 2 It is carried out in saturated 0.1 mol / L KOH. Fig.11 As shown, the results show that it has a relatively high onset potential of 0.63 V and a high current density of 2.5 mA / cm 2 The ORR current density is 0.9 mA / cm 2 The ring current density indicates that there is a large amount of H 2 O 2 generate. Fig.12 H 2 O 2 Selectivity plots show that the catalyst is able to maintain an average of 80% H 2 O 2 Selective. Fig.13 The results show that the number of transferred electrons of the catalyst is close to 2.3, and the ORR pathway is a two-electron pathway to generate H 2 O 2 . Fig.14 The EIS impedance diagram shows that the catalyst has a charge transfer resistance of 32Ω and a high slope in the low-frequency region, indicating that its mass diffusion rate is faster.
[0080] Embodiment 3:
[0081] Example 3 is basically the same Figure 15-17 As shown:
[0082] The difference from the above embodiment is that the etching component includes a solution tank 1, the bottom of the solution tank 1 is fixedly connected by bolts and connected to a nano bubble making machine 2, and a reactor component for etching a Lucien blue analog is arranged in the solution tank 1.
[0083] The reactor assembly includes a reaction vessel 3, a feeding port 4 is opened on the side wall of the reaction vessel 3, a feeding door 5 is hinged on the feeding port 4, a first nano filter plate 6 is vertically slidably fitted on the inner wall of the reaction vessel 3, and a vibration extrusion assembly for extruding and vibrating the Lushi blue analog is provided on the top of the first nano filter plate 6.
[0084] The vibration extrusion assembly includes a slide bar 7, one end of the slide bar 7 is fixedly connected to the top of the first nano filter plate 6 by bolts, the end of the slide bar 7 away from the first nano filter plate 6 is fixedly connected to a spring 8 by bolts, the end of the spring 8 away from the slide bar 7 is fixedly connected to a top cover 9 by bolts, the inner wall of the top cover 9 is symmetrical and integrally formed with triangular sliders 10, and adjacent triangular sliders 10 are arranged in opposite directions; there is an inclined groove 11 on the slide bar 7, a Z-shaped slider 12 is slidably matched in the inclined groove 11, both ends of the Z-shaped slider 12 are slidably matched with adjacent triangular sliders 10, the outer wall of the top cover 9 is slidably matched with a base 13, the outer wall of the base 13 is fixedly connected to a second bracket 21 by bolts, the end of the second bracket 21 away from the base 13 is fixedly connected to the inner wall of the reaction container 3 by bolts, the inner bottom wall of the base 13 is integrally formed with a slide cylinder 14, and the slide cylinder 14 and the base 13 are connected The slide bar 7 penetrates the slide cylinder 14 and vertically slides with the inner wall of the slide cylinder 14. The slide cylinder 14 is provided with a slide groove 15. The Z-shaped slide block 12 and the slide groove 15 are vertically slidably matched; the inner wall of the reaction container 3 is vertically slidably matched with a second nano filter plate 17, and the bottom of the second nano filter plate 17 is fixedly connected with a plurality of support rods 16 by bolts, and the bottoms of the support rods 16 are fixedly connected with the top of the second nano filter plate 17 by bolts; the inner wall of the solution tank 1 is fixedly connected with a first bracket 18 by bolts, and the first bracket 18 is fixedly connected with a funnel 19 at one end away from the inner wall of the solution tank 1 by bolts, the bottom of the funnel 19 penetrates the second nano filter plate 17 and extends to the top of the top cover 9, the bottom of the funnel 19 vertically slides with the part penetrating the second nano filter plate 17, and the part where the bottom of the reaction container 3 is connected to the nano bubble making machine 2 is connected with a one-way valve 20.
[0085] Specific implementation process: ensure that the solution tank 1 is clean and free of impurities, and manually add an appropriate amount of alkaline solution into the solution tank 1 until the alkaline solution covers the top of the reaction container 3.
[0086] The nanobubble making machine 2 is turned on and blows a number of nanometer-sized bubbles into the reaction container 3. The blowing mode is set to blow at intervals of 5 seconds. When the nanobubbles come into contact with the Prussian blue analogue during the rising process, the tail vortex thereof will carry the Prussian blue analogue particles with it to rise together. This carrying effect helps the Prussian blue analogue particles to be dispersed and mixed with KOH in the etching reaction system, so that the Prussian blue analogue particles and KOH are in contact more fully, thereby further improving the purity of the obtained transition metal oxide material.
[0087] The Prussian blue analogue is slowly added from the funnel 19. Since the bottom of the funnel 19 passes through the second nano filter plate 17, the Prussian blue analogue falls from the bottom of the funnel 19 onto the top cover 9 in the reaction vessel 3. The Prussian blue analogue gradually accumulates on the top cover 9. When the Prussian blue analogue reaches a certain weight, the top cover 9 and the base 13 slide vertically together, and the bottom of the top cover 9 and the spring 8 are fixedly connected by bolts. At this time, the weight of the Prussian blue analogue compresses the spring 8, and the top cover 9 slides downward. 9 is fixedly connected by bolts and support rods 16, the support rods 16 and the bottom of the second nano filter plate 17 are fixedly connected by bolts, and at the same time, the second nano filter plate 17 and the bottom of the funnel 19 are vertically slidably matched with the inner wall of the reaction container 3, and the top cover 9 slides downward to drive the second nano filter plate 17 to slide downward. At the same time, since the inner wall of the top cover 9 is symmetrical and integrally formed with a triangular slider 10, both ends of the triangular slider 10 and the Z-shaped slider 12 are slidably matched, the top cover 9 moves downward to make the triangular slider 10 move downward, and at the same time, since the Z-shaped slider 12 is in the slide cylinder 1 4, the Z-shaped slider 12 will move to the right to adapt to the downward movement of the triangular slider 10; because the Z-shaped slider 12 is slidably matched with the inclined groove 11 in the slide bar 7, the slide bar 7 and the slide cylinder 14 are vertically slidably matched, and the rightward movement of the Z-shaped slider 12 will drive the slide bar 7 to move upward. Since the bottom of the slide bar 7 and the first nano filter plate 6 are fixedly connected by bolts, the first nano filter plate 6 and the inner wall of the reaction container 3 are vertically slidably matched, the slide bar 7 will drive the first nano filter plate 6 to move upward, and the first nano filter plate 6 will move upward. The first nano filter plate 6 slides upwards and the second nano filter plate 17 slides downwards, which drives the Prussian blue analogue in the reaction container 3 to be squeezed toward the middle. At this time, the first nano filter plate 6 and the second nano filter plate 17 bring the Prussian blue analogues scattered in various corners together to prevent incomplete reaction of the Prussian blue analogues in some corners. In addition, the nano bubble making machine 2 is set to blow bubbles after the first nano filter plate 6 and the second nano filter plate 17 are brought together, which can greatly change the position of the Prussian blue analogue in the reaction container 3 and improve the reaction effect.
[0088] Since the outer wall of the top cover 9 and the inner wall of the base 13 are vertically slidably matched and in close contact, the top cover 9 can form a seal on the inside of the top cover 9 to avoid the problem of the spring 8 getting stuck due to the Prussian blue analogue entering the inside of the top cover 9.
[0089] During the movement of the Z-shaped slider 12, due to the upper and lower limit effects of the slide groove 15 on the Z-shaped slider 12, the Z-shaped slider 12 always maintains horizontal movement during the movement process. At the same time, the downward movement distance of the top cover 9 is set to be smaller than the downward sliding distance of the Z-shaped slider 12, so that the Z-shaped slider 12 will not cross the bottom of the triangular slider 10.
[0090] At the same time, some of the nanobubbles drive the Prussian blue analogues on the top cover 9. At this time, since the top cover 9 loses part of the weight of the Prussian blue analogues, the spring 8 will recover its deformation when the weight of the Prussian blue particles is reduced. The spring 8 recovers its deformation and drives the top cover 9 to slide upward. The upward sliding of the top cover 9 will drive the second nanofilter plate 17 to slide upward. The upward movement of the top cover 9 causes the triangular slider 10 to move upward. At this time, the Z-shaped slider 12 will move to the left. At this time, the left movement of the Z-shaped slider 12 will drive the slide bar 7 to move downward. At this time, the slide bar 7 will drive the first nanofilter plate 6 to move downward. At this time, the first nanofilter plate 6 slides downward and the second nanofilter plate 17 slides upward to restore to the initial position. Due to the intermittent blowing of nanobubbles and the continuous addition of Prussian blue analogues, the up and down sliding movement of the first nanofilter plate 6 and the second nanofilter plate 17 will be repeated, so that the first nanofilter plate 6 and the second nanofilter plate 17 produce a vibration effect on the internal Prussian blue analogues, and further make the Prussian blue analogue and KOH contact more fully.
[0091] After 10 minutes, the nanobubble making machine 2 is turned off, the KOH is completely extracted, and the Prussian blue analog in the reaction container 3 is taken out from the material taking port 4 to obtain the transition metal oxide.
[0092] The above is only an embodiment of the present invention. The common sense such as the known specific structure and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field know all the common technical knowledge in the technical field of the invention before the application date or priority date, can know all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement this scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for ordinary technicians in the relevant field to implement this application. It should be pointed out that for those skilled in the art, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the patent. The protection scope required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for preparing defect-rich cyanated transition metal oxide material, characterized in that: The following steps are involved: Step 1, preparing a solution: dissolving substance A and substance B in deionized water to obtain solution A and solution B respectively; Step 2, preparing a Prussian blue analog material: stirring and mixing solution A and sodium citrate dihydrate, adding solution B during stirring until a precipitate is precipitated, the stirring time is 24 hours, and the stirred solution is centrifuged and washed 3-10 times with deionized water and anhydrous ethanol, and then the precipitate is filtered and dried to obtain a Prussian blue analog; Step three, prepare a transition metal oxide material rich in oxygen vacancies and surface cyanation: add the obtained Prussian blue analogue to an etching component, add an alkaline solution to the etching component, and etch the Prussian blue analogue in the etching component for 5-10 minutes. Wash the etched Prussian blue analogue with deionized water and anhydrous ethanol for 3-10 times, and dry the washed Prussian blue analogue to obtain a transition metal oxide material rich in oxygen vacancies and surface cyanation.
2. The method for preparing defect-rich cyanated transition metal oxide material according to claim 1, characterized in that: In step 1, substance A includes one or more of Fe(NO3)2, Fe(NO3)3, Co(NO3)2, Ni(NO3)2, Cu(NO3)2, Zn(NO3)2, Mn(NO3)2, FeCl2, FeCl3, CoCl2, NiCl2, CuCl2, ZnCl2 and MnCl2; substance B includes one or more of K3[Fe(CN)6], K4[Fe(CN)6] and K3[Co(CN)6].
3. The method for preparing defect-rich cyanated transition metal oxide material according to claim 2, characterized in that: In step 1, the concentration of solution A is 37.5 mmol / L, and the concentration of solution B is 12.5 mmol / L.
4. The method for preparing defect-rich cyanated transition metal oxide material according to claim 3, characterized in that: In step 2, the mass ratio of sodium citrate dihydrate to solution A is 3.3 g:250 mL, and the volume ratio of solution A to solution B is 1:
1.
5. The method for preparing defect-rich cyanated transition metal oxide material according to claim 4, characterized in that: In step 2, the stirring speed is 200-1000 r / min; the addition rate of solution B is V / 500-V / 100 per minute; The drying treatment is one of vacuum drying treatment and freeze drying treatment. The temperature of the vacuum drying treatment is 60 to 100° C., the temperature of the freeze drying treatment is -35 to -50° C., and the drying treatment time is 10 to 24 hours.
6. The method for preparing defect-rich cyanated transition metal oxide material according to claim 5, characterized in that: In step 3, the mass of the Prussian blue analogue is 750 mg, and the alkaline solution is 50 mL of 0.1 mol / L KOH.
7. A device for preparing defect-rich cyanated transition metal oxide materials, characterized in that: In step three, the etching component comprises a solution tank (1), the bottom of the solution tank (1) is fixedly connected and communicated with a nano bubble making machine (2), and a reactor component for etching a Lushi blue analog is arranged in the solution tank (1).
8. The device for preparing defect-rich cyanated transition metal oxide material according to claim 7, characterized in that: The reactor assembly comprises a reaction container (3), a material taking port (4) is provided on the side wall of the reaction container (3), a material taking door (5) is hinged on the material taking port (4), a first nano filter plate (6) is vertically slidably engaged with the inner wall of the reaction container (3), and a vibration extrusion assembly for extruding and vibrating a Lushi blue analogue is provided on the top of the first nano filter plate (6).
9. The device for preparing defect-rich cyanated transition metal oxide material according to claim 8, characterized in that: The vibration extrusion assembly comprises a slide bar (7), one end of the slide bar (7) is fixedly connected to the top of the first nano filter plate (6), one end of the slide bar (7) away from the first nano filter plate (6) is fixedly connected to a spring (8), one end of the spring (8) away from the slide bar (7) is fixedly connected to a top cover (9), the inner side wall of the top cover (9) is symmetrically and fixedly connected to triangular sliders (10), and adjacent triangular sliders (10) are arranged in opposite directions; an inclined groove (11) is opened in the slide bar (7), a Z-shaped slider (12) is slidably matched in the inclined groove (11), both ends of the Z-shaped slider (12) are slidably matched with adjacent triangular sliders (10), the outer wall of the top cover (9) is slidably matched with a base (13), and the outer wall of the base (13) is fixedly connected to a second bracket ( 21), one end of the second bracket (21) away from the base (13) is fixedly connected to the inner wall of the reaction container (3), the inner bottom wall of the base (13) is fixedly connected with a slide cylinder (14), the slide cylinder (14) and the base (13) are connected, the slide rod (7) passes through the slide cylinder (14) and the base (7) and is vertically slidably matched with the inner wall of the slide cylinder (14) and the base (7), the slide cylinder (14) is provided with a slide groove (15), and the Z-shaped slide block (12) and the slide groove (15) are both vertically slidably matched; the inner wall of the reaction container (3) is vertically slidably matched with a second nano filter plate (17), the bottom of the second nano filter plate (17) is fixedly connected with a plurality of support rods (16), and the bottoms of the support rods (16) are fixedly connected to the top of the second nano filter plate (17).
10. The device for preparing defect-rich cyanated transition metal oxide material according to claim 9, characterized in that: A first bracket (18) is fixedly connected to the inner wall of the solution tank (1); a funnel (19) is fixedly connected to one end of the first bracket (18) away from the inner wall of the solution tank (1); the bottom of the funnel (19) penetrates the second nano filter plate (17) and extends to the top of the top cover (9); the bottom of the funnel (19) and the part penetrating the second nano filter plate (17) are vertically slidably matched; and a one-way valve (20) is connected to the part where the bottom of the reaction container (3) and the nano bubble making machine (2) are connected.
Citation Information
Cited By
Prussian-blue-like catalyst with highly-exposed crystal face (111) and preparation and application of Prussian-blue-like catalyst
CN122214918A