Gas roasting method for starting 500kA aluminum electrolysis cell

The 500kA aluminum electrolytic cell is repaired and calcined by gas calcining method, which solves the problem of uneven heating speed and gradient, improves the working efficiency and the service life of the electrolytic cell, simplifies the startup process and reduces costs.

CN119040962APending Publication Date: 2024-11-29YUNNAN WENSHAN ALUMINUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158572.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When the 500kA aluminum electrolytic cell is started twice or multiple times, the temperature increase speed control is poor, the temperature increase gradient is uneven, resulting in low working efficiency, and the coke grain roasting method is complicated and cumbersome, which increases the labor intensity of workers and may lead to liquid aluminum seepage. leak.

Method used

The gas roasting method is adopted, including repairing the electrolytic tank after the tank is shut down, hanging the anode, laying the cover plate, installing the gas roasting equipment, ignition preparation and maintenance, controlling the roasting temperature until the preset temperature is reached, and powering is turned on.

Benefits of technology

It improves the controllability and gradient uniformity of the heating speed, simplifies the startup process, reduces the labor intensity of workers, extends the service life of the electrolytic cell, and reduces the cost of repair and overhaul.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040962A_ABST
    Figure CN119040962A_ABST
Patent Text Reader

Abstract

The invention provides a gas roasting method for starting a 500kA aluminum electrolysis cell. The gas roasting method comprises the following steps: carrying out corresponding repair treatment on the 500kA aluminum electrolysis cell after the cell is stopped; checking the electrolytic cell, polishing a cathode, and cleaning a hearth and the periphery of the electrolytic cell; checking the gas equipment; adjusting the relative position between the anode and the cathode in the electrolytic cell through the pocket ruler, and hanging the anode; laying a corresponding cover plate on the electrolytic cell; gas roasting equipment corresponding to the electrolytic cell is installed, and corresponding ignition preparation is conducted on the gas roasting equipment; corresponding maintenance treatment is carried out in the roasting process; and after the temperature in the electrolytic cell and the temperature of the furnace bottom reach preset temperature values, the electrolytic cell is electrified, and the problems that when an existing 500kA aluminum electrolytic cell is started for two times or multiple times, the controllability of the temperature rising speed is poor, the temperature rising gradient is uneven, the local temperature is high, the process is tedious and miscellaneous, and the working efficiency is low are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of 500kA aluminum electrolytic cell startup, and in particular to a gas roasting method for starting a 500kA aluminum electrolytic cell. Background Art

[0002] In recent years, affected by the power supply during the flood season and the dry season, 500kA aluminum electrolytic cells have been forced to shut down on a large scale due to power shortages. After the shutdown, they need to be planed and repaired, often facing problems such as severe oxidation of cathode carbon blocks and side blocks. In addition, improper repairs can easily lead to damage to the 500kA aluminum electrolytic cells in the later stage, shortening the service life of the 500kA aluminum electrolytic cells. When the power is sufficient and the conditions for resumption of production are met, the 500kA aluminum electrolytic cells need to be started up twice or more. Therefore, choosing a suitable roasting method is directly related to whether the 500kA aluminum electrolytic cells can be put into production as soon as possible.

[0003] At present, when a 500kA aluminum electrolytic cell is started up for the second or multiple times, the coke particle roasting method is usually used. However, the coke particle roasting method has poor control over the heating rate, and the heating gradient is uneven during the heating process, the local temperature is high, and the heating rate is slow. Complex procedures such as dismantling and laying of coke particles make the whole process cumbersome, resulting in low work efficiency. Moreover, after startup, the carbon slag needs to be salvaged manually, which increases the labor intensity of the workers. The edge fixing paste is not roasted sufficiently, and aluminum liquid leakage is likely to occur after startup. Summary of the invention

[0004] The purpose of the present invention is to provide a gas roasting method for starting a 500kA aluminum electrolytic cell, aiming to solve the problems that the existing 500kA aluminum electrolytic cell has poor controllability over the heating rate when starting for the second or multiple times, and the heating gradient is uneven during the heating process, the local temperature is high, the heating rate is slow, and the complex processes such as dismantling and laying of coke particles make the whole process cumbersome, resulting in low work efficiency, and after starting, the carbon slag needs to be manually salvaged, which increases the labor intensity of the workers, the preheating of the edge fixing paste is not sufficient, and aluminum liquid leakage is easy to occur after starting.

[0005] The embodiments of the present invention are implemented by the following technical solutions:

[0006] A gas roasting method for starting a 500kA aluminum electrolytic cell comprises the following steps:

[0007] a. Perform corresponding repairs on the 500kA aluminum electrolytic cell after it is shut down;

[0008] b. Inspect the repaired 500kA aluminum electrolytic cell, polish the cathode and clean the furnace and the surrounding area of ​​the 500kA aluminum electrolytic cell;

[0009] c. Inspect the gas roasting equipment used for 500kA aluminum electrolytic cells;

[0010] d. Use a ruler to adjust the relative position between the anode and cathode in the 500kA aluminum electrolytic cell after inspection and perform the anode hanging operation;

[0011] e. Lay the corresponding cover plates for the 500kA aluminum electrolytic cells that have completed the anode hanging operation;

[0012] f. Install the gas roasting equipment corresponding to the 500kA aluminum electrolytic cell in step e, and perform corresponding ignition preparation on the gas roasting equipment;

[0013] g. roasting the 500kA aluminum electrolytic cell in step f by using the gas roasting equipment that has completed the ignition preparation, and performing corresponding maintenance during the roasting process;

[0014] h. After the temperature inside the 500kA aluminum electrolytic cell and the temperature at the bottom of the furnace in step g reach the preset temperature values, the 500kA electrolytic cell is powered on.

[0015] Optionally, the specific process of repairing the 500kA aluminum electrolytic cell after the shutdown in step a is as follows:

[0016] According to the side carbon blocks, leg extension and cathode conditions of the 500kA aluminum electrolytic cell after shutdown, corresponding repairs are performed on the corresponding parts of the cell.

[0017] Optionally, in step d, the specific process of adjusting the relative position between the anode and the cathode in the 500kA aluminum electrolytic cell after inspection by using a ruler and performing the anode hanging operation is as follows:

[0018] Before hanging anodes, adjust the gyrometer to 50mm, select 48 qualified anode carbon blocks, and form a group of anodes with four adjacent anode carbon blocks. Determine the highest point of the single-cell cathode surface and the reference leveling line of the first group of anodes. Use a ruler to draw the leveling line of each anode carbon block on the anode guide rod. Place each group of anodes on the cathode surface, draw the anode hanging line on the anode guide rod through a scale plate, and hang anodes according to the anode hanging line. Each group of anodes is alternately arranged on both sides of the horizontal busbar of the 500kA aluminum electrolytic cell. After the anode hanging operation is completed, adjust the gyrometer to 280mm~330mm.

[0019] Optionally, the specific process of laying the corresponding cover plate on the 500kA aluminum electrolytic cell that has completed the anode hanging operation in step e is:

[0020] A first cover plate is laid on the center seam of a 500kA aluminum electrolytic cell that has completed the anode hanging operation, and the gaps between the electrodes are sealed by laying a second cover plate; after adjusting the anode to a preset height, a third cover plate is laid around the anode; a fourth cover plate is laid around the electrolytic cell and on the top of the anode, and the fourth cover plate is insulated and sealed from the edge of the electrolytic cell; a fifth cover plate is arranged at the gas roasting equipment on both sides of the electrolytic cell, the fifth cover plate and the fourth cover plate are arranged crosswise, and the gap between the fifth cover plate and the fourth cover plate is sealed; three exhaust ports are evenly reserved in the center seam of the electrolytic cell, and one exhaust port is reserved at the flue end and the large surface of the electrolytic cell.

[0021] Optionally, the specific process of installing the gas roasting equipment corresponding to the 500kA aluminum electrolytic cell in step e in step f is:

[0022] A burner is installed on the burner installation side of a 500kA aluminum electrolytic cell, with the bottom of the burner being 80 mm to 100 mm away from the cathode surface; an edge panel is installed at the edge of the electrolytic cell, and the edge panel is fixed and sealed; corresponding combustion racks are installed on the edges of both sides of the electrolytic cell, and the combustion racks and the burners are connected by corresponding hoses. After the hoses are connected, the electrolytic cell is sealed, and the combustion racks are numbered and managed; after the sealing of the electrolytic cell is completed, a covering material is installed on the cover plate of the electrolytic cell; a fuel station and a control station are arranged at the aluminum outlet end of the electrolytic cell, corresponding thermocouples are installed, connecting pipelines between the combustion rack and the fuel station are set, air and gas pipelines are connected, and the combustion rack, the fuel station and the control station are connected by quick-connect lines.

[0023] Optionally, the specific process of loading the covering material on the cover plate of the electrolytic cell is:

[0024] A 130 mm thick layer of electrolyte powder is laid on the cover plate, a 100 mm thick layer of electrolyte powder is laid in the middle seam of the electrolytic cell, and a 150 mm to 180 mm thick layer of electrolyte powder is set on the anode as a heat-insulating material.

[0025] Optionally, the particle diameter of the electrolyte powder is 1 mm to 3 mm.

[0026] Optionally, the specific process of performing corresponding ignition preparation on the gas roasting equipment in step f is:

[0027] The temperature rise strategy is set through the control station, and the corresponding roasting time, roasting temperature, gas inlet pipeline pressure value of the gas roasting equipment, gas supply peak value and wind flow rate are set, and the combustion rack gas is exhausted one by one.

[0028] Optionally, in step g, the 500kA aluminum electrolytic cell in step f is roasted by the gas roasting equipment that has completed the ignition preparation, and the specific process of performing corresponding maintenance treatment during the roasting process is:

[0029] The roasting temperature of the 500kA aluminum electrolytic cell is controlled according to the temperature rise gradient requirements. During the roasting process, the roasting temperature is adjusted in time according to the real-time temperature monitored in the furnace.

[0030] Optionally, in step h, after the temperature inside the 500kA aluminum electrolytic cell and the temperature at the bottom of the furnace in step g reach preset temperature values, the specific process of energizing the 500kA electrolytic cell is as follows:

[0031] When the temperature inside the 500kA electrolytic cell reaches the set temperature and the furnace bottom temperature reaches above 50℃, the electrolytic cell is prepared for power-on; one hour before stopping the fire, a non-stop power switch is installed; half an hour before stopping the fire, the combustion air flow and gas flow are set according to the actual situation, the roasting situation is observed, and the thermocouple and the combustion rack control cable are removed; after the roasting is completed, the combustion rack is removed, the burners are removed in sequence, and the installation ports of the burners are sealed. After all the burners are removed, the anode gyrometer is lowered to 60mm~70mm, and inspections are carried out at the same time. The distance between the bottom of the anode and the surface of the cathode is greater than or equal to 3cm; after the anode position is lowered to the specified position, the pre-prepared liquid electrolyte is poured into the electrolytic cell as required, so that the liquid electrolyte soaks the anode for more than 20cm, and the 500kA electrolytic cell is powered on.

[0032] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:

[0033] The present invention provides a gas roasting method for starting a 500kA aluminum electrolytic cell, comprising the following steps: performing corresponding repairing treatment on the 500kA aluminum electrolytic cell after stopping the cell; inspecting the repaired 500kA aluminum electrolytic cell, grinding the cathode and cleaning the furnace and the surroundings of the 500kA aluminum electrolytic cell; inspecting the gas equipment used for the 500kA aluminum electrolytic cell; adjusting the relative position between the anode and the cathode in the inspected 500kA aluminum electrolytic cell by a ruler and performing an anode hanging operation; laying a corresponding cover plate on the 500kA aluminum electrolytic cell after the anode hanging operation is completed; installing gas roasting equipment corresponding to the 500kA aluminum electrolytic cell, and performing corresponding ignition preparation on the gas roasting equipment; roasting the 500kA aluminum electrolytic cell by the gas roasting equipment after the ignition preparation is completed, and performing corresponding maintenance treatment during the roasting process; waiting for 5 After the temperature inside the 100kA aluminum electrolytic cell and the temperature at the bottom of the furnace reach the preset temperature values, the 500kA electrolytic cell is powered on. A corresponding repair method is formulated for each electrolytic cell that needs to be started multiple times, which not only reduces the repair cost, but also reduces the risk of furnace leakage during startup; the gas roasting method is adopted, the heating rate is well controllable, the heating gradient is uniform, the heating rate is fast, and the roasting time is short; the preheating of the edge of the electrolytic cell is more sufficient, which is beneficial to extend the service life of the electrolytic cell; the startup process is simplified, avoiding the installation and disassembly of soft connections and diverters due to coke roasting, and the complicated process of salvaging carbon slag, thereby reducing the workload of workers; there is no problem of bias flow during roasting; while ensuring safe production, the success rate of multiple starts of the electrolytic cell is improved, the repair cost of the electrolytic cell is reduced, and the generation of overhaul waste is reduced, with good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A schematic diagram of a gas roasting process provided in Example 1 of the present invention;

[0035] Figure 2 A schematic diagram of the anode-hanging scribing structure provided in the second embodiment of the present invention;

[0036] Figure 3 This is a schematic diagram of the electrolytic cell structure provided in Example 3 of the present invention. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0038] Embodiment 1

[0039] like Figure 1 As shown, a gas roasting method for starting a 500kA aluminum electrolytic cell comprises the following steps:

[0040] a. Perform corresponding repairs on the 500kA aluminum electrolytic cell after it is shut down;

[0041] b. Inspect the repaired 500kA aluminum electrolytic cell, polish the cathode and clean the furnace and the surrounding area of ​​the 500kA aluminum electrolytic cell;

[0042] c. Check the gas equipment used for 500kA aluminum electrolytic cells;

[0043] d. Use a ruler to adjust the relative position between the anode and cathode in the 500kA aluminum electrolytic cell after inspection and perform the anode hanging operation;

[0044] e. Lay the corresponding cover plates on the 500kA aluminum electrolytic cells that have completed the anode hanging operation;

[0045] f. Install the gas roasting equipment corresponding to the 500kA aluminum electrolytic cell in step e, and perform corresponding ignition preparation on the gas roasting equipment;

[0046] g. roasting the 500kA aluminum electrolytic cell in step f by using the gas roasting equipment that has completed the ignition preparation, and performing corresponding maintenance during the roasting process;

[0047] h. After the temperature inside the 500kA aluminum electrolytic cell and the temperature at the bottom of the furnace in step g reach the preset temperature values, the 500kA electrolytic cell is powered on.

[0048] In this embodiment, the specific process of repairing the 500kA aluminum electrolytic cell after the shutdown in step a is as follows:

[0049] According to the side carbon blocks and leg extension conditions of the 500kA aluminum electrolytic cell after the cell was stopped and the cathode conditions of the electrolytic cell, the corresponding parts of the electrolytic cell were repaired accordingly. Among them, the judgment criteria for the repair method are:

[0050] Standard 1: Determined based on the operation of the electrolytic cell

[0051] For electrolytic cells with an age of ≤2000 days, Si≤0.05%, Fe≤0.2%, and duration ≤30 days, the electrolytic cells that run stably before being shut down can be subjected to minor or medium repairs, otherwise major repairs are required; for electrolytic cells with a furnace bottom temperature ≥200°C and unstable operation before being shut down, major repairs are required.

[0052] Standard 2: Judging by the carbon blocks on the side of the electrolytic cell and the extension of the legs

[0053] For electrolytic cells with intact side carbon blocks and corrosion depth ≤2cm within 8cm below the pressure plate, repair treatment is carried out. The side blocks used for electrolytic cell repair are 90mm thick silicon carbonitride blocks. For electrolytic cells with corrosion depth of side carbon blocks greater than 2cm or cracks in the carbon blocks, the side carbon blocks of the entire cell are replaced. For electrolytic cells with detached or cracked legs, the entire cell is treated with leg paste.

[0054] Standard 3: Determined based on cathode conditions

[0055] For cathodes that remain intact, with cathode lift ≤60mm, cathode carbon gap width ≤10mm, cathode carbon block crack width at its widest ≤5mm, and deepest depth ≤100mm, minor repairs are carried out; for a single group of cathodes with surface peeling depth >100mm, crack width >5mm, and crack depth >100mm, medium repairs are carried out. To ensure the quality of cathode replacement, the cathode must be replaced close to the two ends of the electrolytic cell, the number of cathode groups to be replaced shall not exceed 4 groups, and no more than 3 blocks shall be replaced on one side; for cathodes with hollowing on the surface, the carbon blocks at the hollowing position must be cleaned, and for those with stripping length >2250mm and depth >100mm, major repairs are carried out. The oxide layer on the surface of the cathode carbon blocks that have not been replaced after repair is polished with an angle grinder to remove more than 85% of the oxide layer on the cathode surface.

[0056] Standard 4: Comprehensive situation assessment

[0057] For electrolytic cells with an age of more than 2000 days, damage to the electrolytic cells during operation, deformation height difference of the cathode bottom being greater than 60mm, erosion pit depth of the cathode being ≥100mm, the thinnest part of the cathode carbon block being ≤180mm from the square steel surface, multiple groups of cathodes being broken and having through cracks, severe cathode penetrating aluminum inclusions, and cell shell deformation being ≥12cm, major repairs are required if any of the following eight situations exist.

[0058] After executing the repair method according to the judgment criteria, the risk of damage to the electrolytic cell caused by multiple starts is effectively reduced, the service life of the electrolytic cell is guaranteed, and the maintenance cost is reduced.

[0059] In this embodiment, the specific process of adjusting the relative position between the anode and the cathode in the 500kA aluminum electrolytic cell after inspection by using a ruler and performing the anode hanging operation in step d is as follows:

[0060] Before hanging anodes, adjust the gyrometer to 50mm, select 48 qualified anode carbon blocks, and form a group of anodes with four adjacent anode carbon blocks. First, determine the highest point of the cathode surface of a single electrolytic cell, confirm the reference leveling line of the first group of anodes, and use a ruler to draw the leveling line of each anode carbon block on the anode guide rod. Place each group of anodes on the cathode surface, draw the anode hanging line on the anode guide rod through a scale plate, and hang anodes according to the anode hanging line. Each group of anodes is alternately set on both sides of the horizontal busbar of the 500kA aluminum electrolytic cell. After the anode hanging operation is completed, adjust the gyrometer to 280mm~330mm.

[0061] In this embodiment, the specific process of laying the corresponding cover plate on the 500kA aluminum electrolytic cell that has completed the anode hanging operation in step e is:

[0062] The first cover plate is laid in the middle seam of the 500kA aluminum electrolytic cell that has completed the anode hanging operation. The first cover plate can be a calcium silicate plate with a thickness of 30mm to 50mm. The gaps between the electrodes are sealed by laying the second cover plate, which can be an asbestos plate; after the anode is adjusted to a preset height, the third cover plate is laid around the anode. The third cover plate can be a cover plate with a heat preservation effect to keep the anode warm; the fourth cover plate is laid around the electrolytic cell and on the top of the anode. The fourth cover plate can be an ordinary The fourth cover plate and the edge of the electrolytic cell can be insulated and sealed with asbestos wool; a fifth cover plate is arranged at the gas roasting equipment on both sides of the electrolytic cell, and the fifth cover plate can be a cover plate corresponding to the burner. The fifth cover plate and the fourth cover plate are arranged crosswise, and the gap between the fifth cover plate and the fourth cover plate is sealed; three exhaust ports are evenly reserved in the middle seam of the electrolytic cell, and one exhaust port is reserved at the flue end and the large surface of the electrolytic cell, and the exhaust port diameter is 150mm.

[0063] In this embodiment, the specific process of installing the gas roasting equipment corresponding to the 500kA aluminum electrolytic cell in step e in step f is:

[0064] Burners are installed on both sides of the 500kA aluminum electrolytic cell, and the burners are placed in the burner cover plate. The fixing parts of the burners are adjusted to a suitable position, and the fixing screws are tightened to fix the burners. The bottom of the burner is 80mm to 100mm away from the cathode surface; the groove edge panels are installed at the groove edge of the electrolytic cell. The groove edge panels can be made of cold-rolled plates. The specifications of the groove edge panels can be 2000mm×300mm×1.5mm. The groove edge panels are fixed and sealed; corresponding combustion racks are installed on the groove edges of both sides of the electrolytic cell, and the combustion racks and the burners are connected by corresponding hoses. The hoses are After the pipes are connected, the electrolytic cell is sealed and the combustion rack is numbered and managed; after the sealing of the electrolytic cell is completed, the covering material is installed on the cover plate of the electrolytic cell; the fuel station and the control station are arranged at the aluminum outlet end of the electrolytic cell, the corresponding thermocouples are installed, the connecting pipeline between the combustion rack and the fuel station is set, the air and gas pipelines are connected, and the combustion rack, the fuel station and the control station are connected through quick-connect lines; the power supply can be single-phase 380VAC±10, 50HZ, power 3000VA, which is stable and reliable; the control station is powered on for testing to detect the working condition of the solenoid valve; the cable is insulated for protection.

[0065] In this embodiment, the specific process of installing the covering material on the cover plate of the electrolytic cell is as follows:

[0066] A 130 mm thick layer of electrolyte powder is laid on the cover plate, a 100 mm thick layer of electrolyte powder is laid in the middle seam of the electrolytic cell, and a 150 mm to 180 mm thick layer of electrolyte powder is set on the anode as a heat-insulating material.

[0067] In this embodiment, the particle diameter of the electrolyte powder is 1 mm to 3 mm.

[0068] In this embodiment, the specific process of performing corresponding ignition preparation on the gas roasting equipment in step f is:

[0069] The temperature rise strategy is set through the control station, and the corresponding roasting time, roasting temperature, gas inlet pipeline pressure value of the gas roasting equipment, gas supply peak value and wind flow rate are set, and the combustion rack gas is exhausted one by one.

[0070] In this embodiment, the gas inlet pipeline pressure requirement of the gas roasting equipment is 0.4MPa, and the peak flow rate of the gas supply is required to reach 600NM 3 / H~700NM 3 / H; the temperature rise strategy can be set through the touch screen of the control station. The temperature rise strategy is: the roasting time is set to 80 hours, the middle repair slot can be set to 88 hours, and the roasting temperature is set to 970℃. After setting, read the curve; before ignition, adjust the ignition air flow and gas flow, open the manual valve of the combustion rack air pipeline and manually adjust the air electric valve opening on the touch screen, and control the air flow to 400NM3 / H range, gas flow rate is controlled at 22NM 3 / H range; the gas of the burner racks is drained one by one, all the gas valves of each burner rack are closed, and then the drain valve is opened. The drain time can be set to 5 minutes.

[0071] In this embodiment, in step g, the 500kA aluminum electrolytic cell in step f is roasted by the gas roasting equipment that has completed the ignition preparation, and the specific process of performing corresponding maintenance treatment during the roasting process is as follows:

[0072] The roasting temperature of the 500kA aluminum electrolytic cell is controlled according to the temperature rise gradient requirements. During the roasting process, the roasting temperature is adjusted in time according to the real-time temperature monitored in the furnace. The specific adjustment values ​​are shown in Table 1 and Table 2 below:

[0073] Table 1: Small repair slot roasting temperature gradient setting table

[0074]

[0075]

[0076] Table 2: Equipment table for heating gradient of middle repair trough roasting

[0077] Serial number Set temperature rise (℃) Temperature rise time Total temperature rise time (H) 1 150 4H 4 2 250 12H 16 3 450 15H 31 4 600 14H 45 5 750 12H 57 6 850 11H 68 7 950 12H 80 8 960 4H 84 9 970 4H 88

[0078] In this embodiment, in step h, after the temperature inside the 500kA aluminum electrolytic cell and the temperature at the bottom of the furnace in step g reach the preset temperature values, the specific process of energizing the 500kA electrolytic cell is as follows:

[0079] When the temperature inside the 500kA electrolytic cell reaches the set temperature and the furnace bottom temperature reaches above 50℃, prepare for the electrolytic cell to be powered on; install a non-stop power switch 1 hour before stopping the fire; half an hour before stopping the fire, set the combustion air flow and gas flow according to the actual situation, observe the roasting situation, remove the thermocouple and the combustion rack control cable, and 20 minutes before stopping the fire, shovel the insulation material around the burner to the upper part of the anode to ensure that the burner can be pulled out smoothly; after the roasting is completed, remove the combustion rack, remove the burners in order, and seal the installation port of the burner. Asbestos board or iron plate can be used to seal the installation port. Blockage to reduce heat loss; after all the burners are removed, the anode rotation meter is lowered to 60mm~70mm, and inspections are carried out at the same time. The distance between the bottom of the anode and the surface of the cathode must be greater than or equal to 3cm. Check the anode lifting mechanism to prevent the anode from directly contacting the raised part of the cathode surface; after the anode position is lowered to the specified position, the pre-prepared 20 tons of liquid electrolyte is poured into the electrolytic cell as required. The electrolyte temperature is greater than 950℃, so that the liquid electrolyte soaks the anode for more than 20cm. Before powering on, all short-circuit bolts are tested for looseness and tightness one by one, and then the 500kA electrolytic cell is powered on. Adequate preparations must be made before powering on. The time from the end of the ceasefire to the completion of powering on is controlled within 30 minutes to ensure the electrolyte temperature; after powering on, the voltage is controlled within 10V. When the voltage exceeds 18V, load reduction measures are taken to control safety risks. After powering on, remove the calcium silicate board in the middle seam of the electrolytic cell and the edge insulation cover, add a proper amount of solid electrolyte fragments to the edges of the furnace for insulation, and cover the liquid electrolyte with solid electrolyte fragments, add 1.5 tons of caustic soda, and clean up. During the process of adding materials, contact the tank control to open the automatic NB, and set the NB interval to 120S. Set the electrolytic cell to the operating state and perform RC control.

[0080] Embodiment 2

[0081] Based on the gas roasting method for starting a 500kA aluminum electrolytic cell in Example 1, in this embodiment, the specific process of adjusting the relative position between the anode and the cathode in the 500kA aluminum electrolytic cell after inspection by using a ruler and performing the anode hanging operation is as follows:

[0082] Before hanging the anode, adjust the gyrometer to 50mm, select 48 qualified anode carbon blocks, and each four adjacent anode carbon blocks form a group of anodes. First determine the highest point of the cathode surface of a single electrolytic cell, confirm the reference leveling line of the first group of anodes, and use a ruler to draw the leveling line of each anode carbon block on the anode guide rod. Place each group of anodes on the cathode surface, and draw the anode hanging line on the anode guide rod through the scale plate, such as Figure 2As shown, the anode guide rods numbered 1 to 6 and 19 to 24 are marked with a line 5 cm below the horizontal busbar, the anode guide rods numbered 7 to 10 and 15 to 18 are marked with a line 7 cm below the horizontal busbar, and the anode guide rods numbered 11 to 14 are marked with a line 8 cm below the horizontal busbar. The anode hanging operation is carried out according to the anode hanging line, and each group of anodes is alternately arranged on both sides of the horizontal busbar of the 500kA aluminum electrolytic cell. After the anode hanging operation is completed, the gyrometer is adjusted to 280 mm to 330 mm.

[0083] Embodiment 3

[0084] Based on the gas roasting method for starting a 500kA aluminum electrolytic cell in Example 1, in this embodiment, the specific process of installing the gas roasting equipment corresponding to the 500kA aluminum electrolytic cell in step e is:

[0085] Install the burner on the burner installation side of the 500kA aluminum electrolytic cell, place the burner in the burner cover, adjust the burner fixings to the appropriate position, and tighten the fixing screws to fix the burner. Figure 3 As shown, the burner installation side of the electrolyzer is Figure 3 On both sides of the A and B sides of the electrolytic cell, 12 burner installation areas are respectively arranged on both sides of the A and B sides, corner covers are arranged at the four corners of the electrolytic cell, and end covers are arranged at the ends of the electrolytic cell. Ordinary covers and burner covers are arranged alternately, and several temperature measuring points are arranged on the electrolytic cell to monitor the real-time temperature of the electrolytic cell. The electrolytic cell can be divided into four areas for control, namely control area 1, control area 2, control area 3 and control area 4. The two ends of the electrolytic cell are the aluminum outlet end and the flue end, respectively. The bottom of the burner is 80mm to 100mm away from the cathode surface; a groove edge enclosure is installed at the groove edge of the electrolytic cell. The groove edge enclosure can be made of cold-rolled plates. The specifications of the groove edge enclosure can be 2000mm×300mm×1.5mm. The tank is fixed and sealed along the enclosure; corresponding combustion racks are installed on the tank edges on both sides of the electrolytic cell, and the combustion racks and burners are connected through corresponding hoses. After the hoses are connected, the electrolytic cell is sealed and the combustion racks are numbered and managed; after the sealing of the electrolytic cell is completed, covering materials are installed on the cover plate of the electrolytic cell; the fuel station and the control station are arranged at the aluminum outlet end of the electrolytic cell, the corresponding thermocouples are installed, the connecting pipelines between the combustion rack and the fuel station are set, the air and gas pipelines are connected, and the combustion rack, the fuel station and the control station are connected through quick-connect cables; the power supply can be single-phase 380VAC±10, 50HZ, power 3000VA, which is stable and reliable; the control station is powered on for testing to detect the working condition of the solenoid valve; the cables are heat-insulated.

[0086] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A gas roasting method for starting a 500kA aluminum electrolytic cell, It is characterized in that The following steps are involved: a. Perform corresponding repairs on the 500kA aluminum electrolytic cell after it is shut down; b. Inspect the repaired 500kA aluminum electrolytic cell, polish the cathode and clean the furnace and the surrounding area of ​​the 500kA aluminum electrolytic cell; c. Check the gas equipment used for 500kA aluminum electrolytic cells; d. Use a ruler to adjust the relative position between the anode and cathode in the 500kA aluminum electrolytic cell after inspection and perform the anode hanging operation; e. Lay the corresponding cover plates on the 500kA aluminum electrolytic cells that have completed the anode hanging operation; f. Install the gas roasting equipment corresponding to the 500kA aluminum electrolytic cell in step e, and perform corresponding ignition preparation on the gas roasting equipment; g. roasting the 500kA aluminum electrolytic cell in step f by using the gas roasting equipment that has completed the ignition preparation, and performing corresponding maintenance during the roasting process; h. After the temperature inside the 500kA aluminum electrolytic cell and the temperature at the bottom of the furnace in step g reach the preset temperature values, the 500kA electrolytic cell is powered on.

2. The gas roasting method for starting a 500kA aluminum electrolytic cell according to claim 1, It is characterized in that The specific process of repairing the 500kA aluminum electrolytic cell after the shutdown in step a is as follows: According to the side carbon blocks, leg extension and cathode conditions of the 500kA aluminum electrolytic cell after shutdown, corresponding repairs are performed on the corresponding parts of the cell.

3. The gas roasting method for starting a 500kA aluminum electrolytic cell according to claim 1, It is characterized in that The specific process of adjusting the relative position between the anode and cathode in the 500kA aluminum electrolytic cell after inspection by using a ruler and performing the anode hanging operation in step d is as follows: Before hanging anodes, adjust the gyrometer to 50mm, select 48 qualified anode carbon blocks, and form a group of anodes with four adjacent anode carbon blocks. Determine the highest point of the single-cell cathode surface and the reference leveling line of the first group of anodes. Use a ruler to draw the leveling line of each anode carbon block on the anode guide rod. Place each group of anodes on the cathode surface, draw the anode hanging line on the anode guide rod through a scale plate, and hang anodes according to the anode hanging line. Each group of anodes is alternately arranged on both sides of the horizontal busbar of the 500kA aluminum electrolytic cell. After the anode hanging operation is completed, adjust the gyrometer to 280mm~330mm.

4. The gas roasting method for starting a 500kA aluminum electrolytic cell according to claim 1, It is characterized in that The specific process of laying the corresponding cover plate on the 500kA aluminum electrolytic cell that has completed the anode hanging operation in step e is as follows: A first cover plate is laid on the center seam of a 500kA aluminum electrolytic cell that has completed the anode hanging operation, and the gaps between the anodes are sealed by laying a second cover plate; after the anode is adjusted to a preset height, a third cover plate is laid around the anode; a fourth cover plate is laid around the electrolytic cell and on the top of the anode, and the fourth cover plate is insulated and sealed from the cell edge of the electrolytic cell; a fifth cover plate is arranged at the gas roasting equipment on both sides of the electrolytic cell, the fifth cover plate and the fourth cover plate are arranged crosswise, and the gap between the fifth cover plate and the fourth cover plate is sealed; three exhaust ports are evenly reserved in the center seam of the electrolytic cell, and one exhaust port is reserved at the flue end and the large surface of the electrolytic cell.

5. The gas roasting method for starting a 500kA aluminum electrolytic cell according to claim 1, It is characterized in that The specific process of installing the gas roasting equipment corresponding to the 500kA aluminum electrolytic cell in step e in step f is: A burner is installed on the burner installation side of a 500kA aluminum electrolytic cell, with the bottom of the burner being 80 mm to 100 mm away from the cathode surface; an edge panel is installed at the edge of the electrolytic cell, and the edge panel is fixed and sealed; corresponding combustion racks are installed on the edges of both sides of the electrolytic cell, and the combustion racks and the burners are connected by corresponding hoses. After the hoses are connected, the electrolytic cell is sealed, and the combustion racks are numbered and managed; after the sealing of the electrolytic cell is completed, a covering material is installed on the cover plate of the electrolytic cell; a fuel station and a control station are arranged at the aluminum outlet end of the electrolytic cell, corresponding thermocouples are installed, connecting pipelines between the combustion rack and the fuel station are set, air and gas pipelines are connected, and the combustion rack, the fuel station and the control station are connected by quick-connect lines.

6. The gas roasting method for starting up a 500kA aluminum electrolytic cell according to claim 5, It is characterized in that The specific process of installing the covering material on the cover plate of the electrolytic cell is as follows: A 130 mm thick layer of electrolyte powder is laid on the cover plate, a 100 mm thick layer of electrolyte powder is laid in the middle seam of the electrolytic cell, and a 150 mm to 180 mm thick layer of electrolyte powder is set on the anode as a heat-insulating material.

7. The gas roasting method for starting up a 500kA aluminum electrolytic cell according to claim 6, It is characterized in that The particle diameter of the electrolyte powder is 1 mm to 3 mm.

8. The gas roasting method for starting up a 500kA aluminum electrolytic cell according to claim 1, It is characterized in that The specific process of performing corresponding ignition preparation on the gas roasting equipment in step f is: The temperature rise strategy is set through the control station, and the corresponding roasting time, roasting temperature, gas inlet pipeline pressure value of the gas roasting equipment, gas supply peak value and wind flow rate are set, and the combustion rack gas is exhausted one by one.

9. The gas roasting method for starting a 500kA aluminum electrolytic cell according to claim 1, It is characterized in that In step g, the 500kA aluminum electrolytic cell in step f is roasted by the gas roasting equipment that has completed the ignition preparation. The specific process of performing corresponding maintenance treatment during the roasting process is as follows: The roasting temperature of the 500kA aluminum electrolytic cell is controlled according to the temperature rise gradient requirements. During the roasting process, the roasting temperature is adjusted in time according to the real-time temperature monitored in the furnace.

10. The gas roasting method for starting up a 500kA aluminum electrolytic cell according to claim 1, It is characterized in that In step h, after the temperature inside the 500kA aluminum electrolytic cell and the temperature at the bottom of the furnace in step g reach the preset temperature values, the specific process of energizing the 500kA electrolytic cell is as follows: When the temperature inside the 500kA electrolytic cell reaches the set temperature and the furnace bottom temperature reaches above 50℃, the electrolytic cell is prepared for power-on; one hour before stopping the fire, a non-stop power switch is installed; half an hour before stopping the fire, the combustion air flow and gas flow are set according to the actual situation, the roasting situation is observed, and the thermocouple and the combustion rack control cable are removed; after the roasting is completed, the combustion rack is removed, the burners are removed in sequence, and the installation ports of the burners are sealed. After all the burners are removed, the anode gyrometer is lowered to 60mm~70mm, and inspections are carried out at the same time. The distance between the bottom of the anode and the surface of the cathode is greater than or equal to 3cm; after the anode position is lowered to the specified position, the pre-prepared liquid electrolyte is poured into the electrolytic cell as required, so that the liquid electrolyte soaks the anode for more than 20cm, and the 500kA electrolytic cell is powered on.