Metal composite substrate comprising oxide and single crystal metal layer and preparation method thereof
By growing a single crystal metal thin film on a metal oxide substrate to form a metal composite substrate, the high cost, many defects and conductivity problems in the preparation of pure metal single crystal substrates are solved, and high-quality substrate preparation and simplification are achieved electrical test.
Patent Information
- Application Number
- CN202411156779.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
During the preparation process, existing pure metal single crystal substrates have problems such as high cost, many defects, and electrical conductivity, which makes it difficult for samples to undergo in-situ electronic transport characteristics testing, which affects the quality and operation complexity of two-dimensional materials.
A single crystal metal thin film is grown on it to form a metal composite substrate, and the substrate surface is optimized by thermal annealing and degassing treatment, and a high-quality single crystal metal layer is deposited using magnetron sputtering and other processes.
It realizes high-quality single crystal metal thin film preparation, supports two-dimensional material growth and device preparation, overcomes the conductivity problems, simplifies electrical characteristics testing, and reduces cost and operational complexity.
Smart Images

Figure CN119041016A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a metal composite substrate comprising an oxide layer and a single crystal metal film and a preparation method thereof. Background Art
[0002] Pure metal single crystal substrates such as platinum (Pt), iridium (Ir), copper (Cu), silver (Ag), gold (Au), palladium (Pd) are widely used in basic science, electronic devices, semiconductor manufacturing, catalysis and other fields. For example, in recent years, various two-dimensional materials such as graphene and molybdenum disulfide have attracted much attention due to their unique electronic band structure and excellent performance, providing a broad platform for the development and application of new electronic devices. Pure metal single crystal substrates such as platinum (Pt), iridium (Ir), copper (Cu), silver (Ag), gold (Au), palladium (Pd) are commonly used substrates for growing single-layer or multi-layer two-dimensional materials. In addition, pure metal single crystal substrates are also commonly used to grow single atomic layer materials. At present, the mainstream methods for producing single crystal metal substrates are the Czochralski method and the Bridgman method. On the one hand, since pure metal single crystal substrates are made of metal as a whole, the cost is relatively high when some precious metals are involved. On the other hand, the metal single crystals prepared by these two methods inevitably have defects visible to the naked eye, such as black spots, tiny bubbles, etc., and the crystals themselves will also have common defects in metal single crystals, such as dislocations, twins, stacking faults, etc. The produced metal single crystal substrates also need to undergo processes such as grinding and polishing, which may damage the surface crystal structure of the substrate. These defects may affect the subsequent use of pure metal single crystal substrates, for example, they will have a negative impact on the quality of the two-dimensional materials grown thereon. Therefore, pure metal single crystal substrates with higher quality requirements are currently mainly dependent on imports, which further increases costs. In addition, since pure metal single crystal substrates are inherently conductive, samples prepared on them cannot be tested for in-situ electron transport properties due to substrate shunting, but need to be transferred to an insulating substrate before testing, which increases the complexity of the operation.
[0003] Therefore, how to provide high-quality metal substrates to overcome the above-mentioned deficiencies remains a problem to be solved urgently. Summary of the invention
[0004] The present invention is proposed in view of the above problems.
[0005] The present invention proposes a metal composite substrate to replace the current pure metal single crystal substrate. The metal composite substrate can use a metal oxide material as a base layer, and grow a single crystal metal film thereon to form a composite substrate. The method proposed by the present invention can prepare high-quality single crystal metal films, which can be used to grow / epitaxially a single layer, a multi-layer two-dimensional material or a single atomic layer material thereon, and can also use the single crystal metal film as a reaction material itself to prepare a two-dimensional material. For example, a single crystal Pt film grown on a metal oxide substrate can form a PtTe crystal layer together with a tellurium source through a chemical vapor deposition (CVD) process.
[0006] According to one embodiment, a method for preparing a metal composite substrate is provided, comprising: providing a single crystal metal oxide substrate; performing a thermal annealing treatment on the metal oxide substrate in an oxygen atmosphere; heating the metal oxide substrate in a vacuum environment for a degassing treatment; and depositing a single crystal metal layer on the metal oxide substrate.
[0007] In one embodiment, the metal oxide substrate comprises at least one of the following materials: Al2O3, MgO, SrTiO3, SrRuO3, BaTiO3, KTaO3, LaAlO3, LaSrAlTaO3, MgAl2O4, LiTaO3, Gd3Ga5O 12 、Gd3Sc2Ga3O 12 , Gd 0.63 Y 2.37 Sc2Ga3O 12 、Y3Sc2Ga3O 12 、Y3Fe5O 12 , YAlO3, ScMgAlO4. Preferably, the metal oxide substrate may include Al2O3, MgO, SrTiO3, SrRuO3, BaTiO3, KTaO3, LaAlO3, LaSrAlTaO3, MgAl2O4, Gd3Ga5O 12 One of, or more preferably includes one of Al2O3, MgO, SrTiO3, KTaO3, LaAlO3, LaSrAlTaO3.
[0008] In one embodiment, the thermal annealing treatment is performed at a first temperature, and the degassing treatment is performed at a second temperature, the second temperature being lower than the first temperature. The first temperature may be in the range of 800° C. to 1200° C., preferably in the range of 950° C. to 1100° C. The second temperature may be in the range of 400° C. to 900° C., preferably in the range of 500° C. to 800° C., and more preferably in the range of 600° C. to 700° C.
[0009] In one embodiment, the process of depositing the single crystal metal layer on the metal oxide substrate is selected from one of the following processes: magnetron sputtering, molecular beam epitaxy, electron beam evaporation, high frequency induction evaporation, pulsed laser deposition, atomic layer deposition, laser evaporation, thermal chemical vapor deposition, plasma chemical vapor deposition, metal chemical vapor deposition. Among them, magnetron sputtering, molecular beam epitaxy, electron beam evaporation, pulsed laser deposition, atomic layer deposition, and metal chemical vapor deposition are preferred, and magnetron sputtering is most preferred.
[0010] In one embodiment, the single crystal metal layer includes at least one of the following materials: Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Rh, Ru, Re, Ta, W, Ti, Al, Bi, Cr, Sb, Cd, Co, Dy, Gd, Ge, Hf, Ho, In, Fe, Pb, Ni, V, Y, Zn, Zr, preferably includes at least one of Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Rh, Ru, Re, Ta, W, Ti, Al, Bi, Cr, more preferably includes at least one of Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Ta, W, Ti.
[0011] In one embodiment, the surface roughness of the metal oxide substrate is less than 2 nm, preferably less than 1 nm, more preferably less than 0.5 nm. The crystal orientation tolerance of the metal oxide substrate is less than 2°, preferably less than 1°, more preferably less than 0.5°.
[0012] According to one embodiment, a metal composite substrate prepared according to the above method is provided, comprising: a single crystal metal oxide substrate; and a single crystal metal layer formed on the metal oxide substrate.
[0013] In one embodiment, the metal oxide substrate comprises at least one of the following materials: Al2O3, MgO, SrTiO3, SrRuO3, BaTiO3, KTaO3, LaAlO3, LaSrAlTaO3, MgAl2O4, LiTaO3, Gd3Ga5O 12 、Gd3Sc2Ga3O 12 , Gd 0.63 Y 2.37 Sc2Ga3O 12 、Y3Sc2Ga3O 12 、Y3Fe5O 12 , YAlO3, ScMgAlO4. Preferably, the metal oxide substrate may include Al2O3, MgO, SrTiO3, SrRuO3, BaTiO3, KTaO3, LaAlO3, LaSrAlTaO3, MgAl2O4, Gd3Ga5O 12One of, or more preferably includes one of Al2O3, MgO, SrTiO3, KTaO3, LaAlO3, LaSrAlTaO3.
[0014] In one embodiment, the single crystal metal layer includes at least one of the following materials: Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Rh, Ru, Re, Ta, W, Ti, Al, Bi, Cr, Sb, Cd, Co, Dy, Gd, Ge, Hf, Ho, In, Fe, Pb, Ni, V, Y, Zn, Zr, preferably includes at least one of Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Rh, Ru, Re, Ta, W, Ti, Al, Bi, Cr, more preferably includes at least one of Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Ta, W, Ti. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Schematic diagram of the structure of a metal composite substrate according to an embodiment of the present invention.
[0016] Figure 2 is a flow chart of a method for preparing a metal composite substrate according to an embodiment of the present invention.
[0017] Figure 3 This is an atomic force microscope photo of an Al2O3 substrate that has been thermally annealed.
[0018] Figure 4 1 is an X-ray diffraction diagram of a metal composite substrate including an Al2O3 substrate and a single crystal Pt layer prepared according to an embodiment of the present invention.
[0019] Figure 5 3 is a transmission electron microscope photograph of a metal composite substrate including an Al2O3 substrate and a single crystal Pt layer prepared according to an embodiment of the present invention.
[0020] Figure 6 3 is a low energy electron diffraction pattern of a metal composite substrate including an Al2O3 substrate and a single crystal Pt layer prepared according to an embodiment of the present invention.
[0021] Figure 7 The PtTe is formed on the metal composite substrate according to one embodiment of the present invention. 1.75 Low-energy electron diffraction pattern of two-dimensional materials.
[0022] Figure 8 The PtTe is formed on the metal composite substrate according to one embodiment of the present invention. 1.75 Scanning tunneling microscopy image of a two-dimensional material.
[0023] Fig. 9The schematic diagram is a structural diagram of a microwave device for performing spin torque-ferromagnetic resonance measurement formed on a metal composite substrate according to an embodiment of the present invention.
[0024] Fig.10 Yes Fig. 9 Schematic diagram of the ferromagnetic resonance signal generated by the electron spin torque obtained by measuring the microwave device shown.
[0025] Fig.11 Yes Fig. 9 The microwave device shown is measured to obtain the relationship curve between the voltage and the external magnetic field when ferromagnetic resonance occurs. DETAILED DESCRIPTION
[0026] Exemplary embodiments of the present invention are described below with reference to the accompanying drawings.
[0027] Figure 1 FIG. 1 is a schematic diagram showing the structure of a metal composite substrate 100 according to an embodiment of the present invention. Figure 1 As shown, the metal composite substrate 100 may include a metal oxide substrate 110 and a single crystal metal layer 120 formed on the metal oxide substrate 110 .
[0028] The metal oxide substrate 110 also has a single crystal structure, so as to form a metal layer 120 of a single crystal structure thereon, which will be discussed in detail below. It is understood that the metal oxide material used to form the metal oxide substrate 110 can be selected according to the material of the single crystal metal layer 120 to be formed so that the lattice constants of the two are matched or close to each other. In some embodiments, the metal oxide substrate 110 may include at least one of the following materials: Al2O3, MgO, SrTiO3, SrRuO3, BaTiO3, KTaO3, LaAlO3, LaSrAlTaO3, MgAl2O4, LiTaO3, Gd3Ga5O 12 、Gd3Sc2Ga3O 12 , Gd 0.63 Y 2.37 Sc2Ga3O 12 、Y3Sc2Ga3O 12 、Y3Fe5O 12 , YAlO3, ScMgAlO4. It should be understood that these materials are given as examples only, and the present invention is not limited to these exemplary materials. Preferably, the metal oxide substrate 110 may include Al2O3, MgO, SrTiO3, SrRuO3, BaTiO3, KTaO3, LaAlO3, LaSrAlTaO3, MgAl2O4, Gd3Ga5O 12One of, or more preferably includes one of Al2O3, MgO, SrTiO3, KTaO3, LaAlO3, LaSrAlTaO3, these preferred materials can be formed into a good and stable single crystal structure using the existing pulling method or crucible lowering method (i.e., Bridgman method), so as to form a metal layer 120 with a good single crystal structure thereon.
[0029] The single crystal metal layer 120 may include any suitable metal material, for example, an appropriate metal material may be selected according to the purpose of the composite substrate 100. In some embodiments, the single crystal metal layer 120 may include at least one of the following materials: Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Rh, Ru, Re, Ta, W, Ti, Al, Bi, Cr, Sb, Cd, Co, Dy, Gd, Ge, Hf, Ho, In, Fe, Pb, Ni, V, Y, Zn, Zr. Preferably, the single crystal metal layer 120 may include at least one of Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Rh, Ru, Re, Ta, W, Ti, Al, Bi, Cr, or more preferably at least one of Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Ta, W, Ti. These preferred materials are often used to grow single-layer or multi-layer two-dimensional materials thereon, such as graphene, molybdenum disulfide, copper disulfide, indium selenide, etc., or to grow single-atomic layer or multi-atomic layer materials with specific crystal orientation, such as growing ferromagnetic materials with perpendicular anisotropy, etc.
[0030] Figure 2 FIG. 2 is a flow chart of a method 200 for preparing a metal composite substrate 100 according to an embodiment of the present invention. Figure 2 As shown, the method 200 may include step 210, providing a single crystal metal oxide substrate 110. The single crystal metal oxide substrate 110 may be commercially purchased, or may be prepared by a Czochralski method, a crucible descent method, or other suitable methods. It should be understood that the strength of the ionic bond in the metal oxide is much higher than the strength of the metal bond between metal atoms in the pure metal, and the single crystal metal oxide can be formed in an oxygen atmosphere or an atmospheric atmosphere, so it is easier to form a high-quality single crystal metal oxide substrate 110 compared to a single crystal pure metal material. In one embodiment, the surface roughness of the provided metal oxide substrate 110 is less than 2 nm, preferably less than 1 nm, and more preferably less than 0.5 nm, and the crystal orientation tolerance of the provided metal oxide substrate 110 is less than 2°, preferably less than 1°, and more preferably less than 0.5°.
[0031] Next, in step 220, the single crystal metal oxide substrate 110 may be subjected to a high temperature thermal annealing treatment. The annealing treatment may be performed in an oxygen atmosphere, and the temperature may be high enough to promote atomic reconstruction on the surface of the metal oxide substrate to form a step structure. It is understood that the annealing temperature should be lower than the melting point of the metal oxide. An appropriate annealing temperature may be selected according to the material of the metal oxide, generally in the range of 800°C to 1200°C, preferably in the range of 950°C to 1100°C. The annealing time may be in the range of 0.5 hours to 24 hours, preferably in the range of 1 hour to 6 hours. The annealed single crystal metal oxide substrate 110 may be naturally cooled to about room temperature in an oxygen atmosphere.
[0032] Continue to refer to Figure 2 In step 230, the annealed single crystal metal oxide substrate 110 can be transferred to a vacuum chamber for depositing the single crystal metal layer 120, and before depositing the single crystal metal layer 120, the single crystal metal oxide substrate 110 is first subjected to a low temperature heating degassing treatment. It should be understood that the "low temperature" here is relative to the "high temperature" used to perform the annealing treatment in step 220, that is, the heating temperature of the degassing treatment is lower than the heating temperature of the annealing treatment. In some embodiments, the heating temperature of the degassing treatment can be in the range of 400°C to 900°C, preferably in the range of 500°C to 800°C, and more preferably in the range of 600°C to 700°C. The heating time is 5 minutes to 2 hours, preferably 10 minutes to 1 hour. The vacuum environment for the degassing treatment can be 10 -4 Pa or less, more preferably 10 -6 The degassing treatment can remove gas molecules attached to the substrate surface, thereby facilitating providing a clean surface with a good crystal structure for depositing the single crystal metal layer 120 thereon.
[0033] In step 240, a single crystal metal layer 120 may be deposited on the metal oxide substrate 110. Various suitable methods may be used to deposit the single crystal metal layer 120, examples of which include but are not limited to magnetron sputtering, molecular beam epitaxy, electron beam evaporation, high frequency induction evaporation, pulsed laser deposition, atomic layer deposition, laser evaporation, thermal chemical vapor deposition, plasma chemical vapor deposition, metal chemical vapor deposition, etc. Among them, magnetron sputtering, molecular beam epitaxy, electron beam evaporation, pulsed laser deposition, atomic layer deposition, and metal chemical vapor deposition are preferred, and magnetron sputtering is most preferred. It is understood that, depending on the process used, appropriate process parameters may be used to form the single crystal metal layer 120. Taking magnetron sputtering as an example, the relevant process parameters may be, for example: the background vacuum is less than or equal to 8×10 -6 Pa, preferably less than or equal to 8×10 -7Pa; the heating temperature of the oxide substrate is 400°C-900°C, preferably 500°C-800°C, and more preferably 600°C-700°C; the sputtering power is 5-100W, preferably 5-20W, and more preferably 5-10W; the argon gas flow rate can be about 100sccm; the chamber pressure during sputtering is about 1.15×10 -2 Pa. It should be understood that the relevant process parameters can be appropriately adjusted according to the metal material to be sputter-deposited.
[0034] An example of using the method 200 to prepare a metal composite substrate is described below.
[0035] Example 1
[0036] Provide Al2O3 (0001) substrate, use tubular annealing furnace to anneal Al2O3 substrate, the back vacuum is 5×10 - 4 Pa, oxygen flow rate is 100 sccm, and the vacuum degree after oxygen is passed is 1×10 -1 Pa, the annealing temperature is about 1020℃, and the annealing time is about 5 hours. The Al2O3 (0001) substrate after annealing is observed using an atomic force microscope (AFM). Figure 3 As shown, it can be seen that the substrate surface has regular atomic-level steps, which provides a good crystal surface for the subsequent deposition of high-quality single-crystalline metal layers.
[0037] The annealed Al2O3 (0001) substrate was transferred to the vacuum chamber of the magnetron sputtering equipment. The Al2O3 (0001) substrate was first heated to about 600°C in the vacuum chamber for about 30 minutes to perform degassing. After degassing, a single crystal Pt metal layer was sputtered on the Al2O3 (0001) substrate. The sputtering process was as follows: the back vacuum of the magnetron sputtering was 8×10 -7 Pa, the distance between the target and the substrate is 15 cm, the argon flow rate is 75 sccm, the sputtering power is 10 W, and the pressure after the argon gas is passed during sputtering is 1.15×10 -2 Pa, the deposition rate of Pt on the substrate is about 0.15 nm / s, and the temperature of the Al2O3 (0001) substrate is maintained at about 640°C during sputtering. After sputtering, the substrate is maintained at about 640°C for 1 hour for in-situ annealing.
[0038] Figure 4 is an X-ray diffraction (XRD) pattern of the Al2O3 / Pt composite substrate prepared in Example 1, which shows a diffraction peak corresponding to Pt(111). Figure 5 This is a high-resolution transmission electron microscope (TEM) photograph of the Pt metal layer on the Al2O3 / Pt composite substrate of Example 1. It can be seen that the Pt metal layer has a very high-quality single crystal structure. Figure 6 Figure 1 is a low energy electron diffraction (LEED) photograph of the Pt metal layer on the Al2O3 / Pt composite substrate of Example 1, showing the atomic arrangement structure of the crystal surface. Figure 6 It can be seen that Pt atoms are regularly arranged in a single crystal structure. Figures 4 to 6 The measurement results show that a high-quality Pt (111) single crystal metal layer was prepared in Example 1.
[0039] The single crystal metal layer 120 of the metal composite substrate 100 prepared according to the present invention can be used as a seed layer or a buffer layer to form additional layers thereon, such as a single layer or multiple layers of a two-dimensional material, or a single atomic layer or multiple atomic layers of a non-two-dimensional material. The following describes the formation of a two-dimensional material PtTe on the Al2O3 / Pt composite substrate of Example 1. 1.75 Instance of .
[0040] Example 2
[0041] Molecular beam epitaxy (MBE) technology was used to grow a single layer of Te on the Al2O3 / Pt composite substrate in Example 1. The process parameters were as follows: -8 The Al2O3 / Pt composite substrate was heated and degassed in a vacuum chamber of 1.5 Pa at a temperature of 500°C for 3 hours. The Pt single crystal metal film on the Al2O3 / Pt composite substrate was sputtered and annealed to obtain an atomically flat surface. The sputtering voltage was 800 V, the beam current was 10 mA, and the sputtering argon pressure was 1×10 -3 Pa, the sputtering time is 15 minutes; then annealing is performed, the annealing temperature is 500°C, the annealing time is 1 hour, and the composite substrate is cooled to room temperature after annealing; Te particles with a purity of 99.99% are used as evaporation source materials, the evaporation temperature is 300°C, and the evaporation source is preheated for 30 minutes before evaporation to ensure beam stability, keep the composite substrate near room temperature, and grow a Te layer on the single crystal Pt layer for 300 seconds.
[0042] Then, the composite substrate with the Te layer grown thereon is subjected to thermal annealing, and the Pt layer and the Te layer form a PtTe 1.75 Alloy layer. The annealing temperature is 400°C and the annealing time is 1 hour. Figure 7 The formed PtTe 1.75 Low energy electron diffraction (LEED) pattern of the layer, Figure 8 The scanning tunneling microscope (STM) photo is shown. Figure 7 and Figure 8 The measurement results confirmed that the electron diffraction spots of PtTe were sharp and the atomic resolution was clear. 1.75 Single crystal sample.
[0043] Since the metal composite substrate of the present invention includes an insulating metal oxide substrate, the single crystal metal film thereon can be etched into a desired device shape to perform relevant electrical characteristic measurements, which overcomes the difficulty of performing electrical measurements on a traditional pure metal substrate due to overall conductivity. An example of performing relevant measurements is discussed below.
[0044] Example 3
[0045] In this example, spin torque-ferromagnetic resonance (STFMR) measurements were performed on the samples obtained in Example 2 to characterize the PtTe 1.75 In order to perform STFMR measurements, it is necessary to 1.75 A ferromagnetic layer is further grown on the layer. The specific method is as follows: a physical vapor deposition process is adopted, and a Fe wire with a purity of 99.999% is used as the source material. It is placed in a Ta boat as an evaporation source, and the evaporation source is heated to about 900°C. It is preheated for 30 minutes to ensure the stability of the beam, and then vapor deposition is performed. The growth thickness is monitored by a film thickness meter to be 6nm. Then, Au particles with a purity of 99.999% are used as the source material, and the evaporation source is heated to 1200°C to grow an Au layer on the Fe layer as an anti-oxidation protective layer. Before growth, the evaporation source is preheated for 30 minutes to ensure the stability of the beam, and the growth film thickness is monitored by a film thickness meter to be 2nm. Using micro-nano processing methods, such as photolithography and etching, the sample is processed into a spin torque-ferromagnetic resonance (STFMR) microwave device, such as Fig. 9 As shown in the reference numeral 40 in FIG. 1 , it includes PtTe 1.75 / Fe / Au structure. It should be noted that etching should be carried out all the way to the insulating metal oxide base layer to ensure that PtTe 1.75 Then, electrodes for measurement can be formed at both ends of the microwave device, including electrodes 10 and 30 led out from one end, and electrode 20 led out from the other end, as shown in FIG. Fig. 9 During measurement, a GSG probe can be used to contact the electrodes 10, 20 and 30 respectively to measure microwave signals. Fig.10 This is a graph of the ferromagnetic resonance signal generated by the electron spin torque measured for this sample. Fig.10 As shown, the sample undergoes ferromagnetic resonance at a magnetic field of about 500 Oe, corresponding to the minimum value of the voltage. Fig.11 This is a curve chart of the voltage change caused by the change in microwave photoresistance when ferromagnetic resonance occurs, measured for the sample. Fig.11As shown, there is a dependence between the voltage value and the direction of the external magnetic field (i.e., the angle between the external magnetic field and the current). Through these tests, it can be seen that when the composite substrate of the present invention is used instead of the traditional pure metal substrate, the overall conductivity problem of the pure metal substrate can be overcome, and the material formed on the substrate can be conveniently tested electrically without, for example, transferring the material to an insulating substrate.
[0046] It should be understood that Example 2 and Example 3 described above are merely application examples of the composite substrate of the present invention, and the composite substrate of the present invention can also be used in various other scenarios instead of the traditional pure metal substrate.
[0047] Unless the context clearly requires otherwise, throughout the specification and claims, the words "comprise", "comprising", "including", "comprising", etc. should be interpreted in an inclusive sense, rather than an exclusive or exhaustive sense. That is, the meaning is "including but not limited to". The word "connected" as generally used herein refers to two or more elements that can be directly connected or connected through one or more intermediate elements. As generally used herein, the word "connected" refers to two or more elements that can be directly connected or connected through one or more intermediate elements. In addition, when used in this application, the words "herein", "above", "below" and words of similar meanings should refer to the entirety of this application rather than to any particular part of this application. Where the context permits, the word "or" refers to a list of two or more items, which covers all of the following interpretations of the word: any item in the list, all items in the list, and any combination of items in the list.
[0048] Furthermore, unless otherwise specifically stated or understood in the context of use, conditional language used herein, such as "can," "may," "might," "could," "for example," "for example," "such as," and the like, is generally intended to convey that certain embodiments include, while other embodiments do not include, certain features, elements, and / or states. Thus, such conditional language is generally not intended to imply that one or more embodiments require features, elements, and / or states in any way, or that one or more embodiments must include logic for making decisions, with or without author input or prompting, that such features, elements, and / or states are included or will be performed in any particular embodiment.
[0049] Although certain embodiments have been described, these embodiments are presented only by way of example and are not intended to limit the scope of the present disclosure. In fact, the novel facilities, methods, and systems described herein may be embodied in various other forms; in addition, various omissions, substitutions, and changes may be made to the forms of the methods and systems described herein without departing from the spirit of the present disclosure. For example, although blocks are presented in a given arrangement, alternative embodiments may perform functions similar to different components and / or circuit topologies, and may delete, move, add, subdivide, combine, and / or modify some blocks. Each of these blocks may be implemented in a variety of different ways. Any suitable combination of the elements and actions of the various embodiments described above may be combined to provide further embodiments. The attached claims and their equivalents are intended to cover these forms or modifications that fall within the scope and spirit of the present disclosure.
[0050] The above description has been given for the purpose of illustration and description. In addition, this description is not intended to limit the embodiments of the present invention to the forms disclosed herein. Although a number of example aspects and embodiments have been discussed above, those skilled in the art will recognize certain variations, modifications, changes, additions and sub-combinations thereof.
Claims
1. A method for preparing a metal composite substrate, comprising: providing a single crystal metal oxide substrate; performing a thermal annealing treatment on the metal oxide substrate in an oxygen atmosphere; heating the metal oxide substrate in a vacuum environment to perform a degassing process; A single crystal metal layer is deposited on the metal oxide substrate.
2. The method of claim 1, wherein: The metal oxide substrate comprises at least one of the following materials: <h2 style=";text-align:left;direction:ltr">Al2O3、MgO、SrTiO3、SrRuO3、BaTiO3、KTaO3、LaAlO3、LaSrAlTaO3、MgAl2O4、LiTaO3、Gd3Ga5O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Gd3Sc2Ga3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Gd<h2 style=";text-align:left;direction:ltr"> 0.63 <h2 style=";text-align:left;direction:ltr"> Y<h2 style=";text-align:left;direction:ltr"> 2.37 <h2 style=";text-align:left;direction:ltr"> Sc2Ga3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Y3Sc2Ga3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Y3Fe5O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> 、YAlO3、ScMgAlO4。 3. The method of claim 1, wherein: The thermal annealing process is performed at a first temperature, and the degassing process is performed at a second temperature, which is lower than the first temperature.
4. The method of claim 3, wherein: The first temperature is in the range of 800°C to 1200°C, preferably in the range of 950°C to 1100°C, The second temperature is in the range of 400°C to 900°C, preferably in the range of 500°C to 800°C, and more preferably in the range of 600°C to 700°C.
5. The method of claim 1, wherein: The process of depositing a single crystal metal layer on the metal oxide substrate is selected from one of the following processes: Magnetron sputtering, molecular beam epitaxy, electron beam evaporation, high frequency induction evaporation, pulsed laser deposition, atomic layer deposition, laser evaporation, thermal chemical vapor deposition, plasma chemical vapor deposition, metal chemical vapor deposition.
6. The method of claim 1, wherein: The single crystal metal layer includes at least one of the following materials: Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Rh, Ru, Re, Ta, W, Ti, Al, Bi, Cr, Sb, Cd, Co, Dy, Gd, Ge, Hf, Ho, In, Fe, Pb, Ni, V, Y, Zn, Zr.
7. The method of claim 1, wherein: The surface roughness of the metal oxide substrate is less than 2 nm, preferably less than 1 nm, more preferably less than 0.5 nm, and The crystal orientation tolerance of the metal oxide substrate is less than 2°, preferably less than 1°, and more preferably less than 0.5°.
8. A metal composite substrate prepared according to the method according to any one of claims 1 to 7, comprising: Single crystal metal oxide substrate; as well as A single crystal metal layer is formed on the metal oxide substrate.
9. The metal composite substrate according to claim 8, wherein: The metal oxide substrate comprises at least one of the following materials: <h2 style=";text-align:left;direction:ltr">Al2O3、MgO、SrTiO3、SrRuO3、BaTiO3、KTaO3、LaAlO3、LaSrAlTaO3、MgAl2O4、LiTaO3、SiC、Gd3Ga5O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Gd3Sc2Ga3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Gd<h2 style=";text-align:left;direction:ltr"> 0.63 <h2 style=";text-align:left;direction:ltr"> Y<h2 style=";text-align:left;direction:ltr"> 2.37 <h2 style=";text-align:left;direction:ltr"> Sc2Ga3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Y3Sc2Ga3O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> Y3Fe5O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> 、YAlO3、ScMgAlO4。 10. The metal composite substrate according to claim 8, wherein: The single crystal metal layer includes at least one of the following materials: Pt, Ir, Cu, Ag, Au, Pd, Nb, Mo, Rh, Ru, Re, Ta, W, Ti, Al, Bi, Cr, Sb, Cd, Co, Dy, Gd, Ge, Hf, Ho, In, Fe, Pb, Ni, V, Y, Zn, Zr.