Compound lead phosphate fluoride, lead phosphate fluoride nonlinear optical frequency doubling crystal, and preparation method and application of compound lead phosphate fluoride nonlinear optical frequency doubling crystal

Through the preparation and optimization growth method of compound fluoride lead phosphate PbPO3F, the problem of difficulty in growing existing short-wavelength nonlinear optical frequency doubling crystals is solved, and high-quality large-size crystals are obtained, which realizes effective application in optical devices.

CN119041026AActive Publication Date: 2024-11-29BEIJING NORMAL UNIV AT ZHUHAI

Patent Information

Application Number
CN202410987070.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-29
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing short-wavelength nonlinear optical frequency doubling crystals, such as KBe2BO3F2, BaB2O4 and LiB3O5, are difficult to grow large-sized crystals and have a small birefringence, which limits their application.

Method used

Preparation by solid-phase reaction method or solution method of compound fluorinated lead phosphate PbPO3F, large-size nonlinear optical frequency doubling crystals are grown by melt method, vacuum encapsulation method, hydrothermal method or room temperature solution volatilization method, and the growth conditions of the crystals are optimized. To obtain high quality PbPO3F crystals.

Benefits of technology

Successfully obtained a large-size, transparent and stable PbPO3F nonlinear optical frequency multiplication crystal, which has the advantages of fast growth speed, low cost and easy to obtain large-size crystals. It also performs 2-fold and 3-fold harmonics in the fundamental frequency light of 1064nm. Light output, suitable for producing short wavelength frequency multiplier optical output of 266nm and other optics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041026A_ABST
    Figure CN119041026A_ABST
Patent Text Reader

Abstract

The invention discloses a compound fluorinated lead phosphate and a fluorinated lead phosphate nonlinear optical frequency doubling crystal as well as a preparation method and application thereof, and belongs to the technical field of nonlinear optical frequency doubling crystals, the chemical formula of the compound fluorinated lead phosphate is PbPO3F, the molecular weight is 305.16, and the compound fluorinated lead phosphate is prepared by adopting a solid-phase synthesis method or a solution method; the chemical formula of the fluorinated lead phosphate nonlinear optical frequency doubling crystal is PbPO3F, the molecular weight of the fluorinated lead phosphate nonlinear optical frequency doubling crystal is 305.16, the fluorinated lead phosphate nonlinear optical frequency doubling crystal belongs to an orthorhombic system, the space group of the fluorinated lead phosphate nonlinear optical frequency doubling crystal is Cc, the cell parameters of the fluorinated lead phosphate nonlinear optical frequency doubling crystal are as follows: alpha = 90 degrees, beta = 126.0920 (10) degrees and gamma = 90 degrees, and the unit cell volume of the fluorinated lead phosphate nonlinear optical frequency doubling crystal is # imgabs0 # imgabs1 #; the frequency doubling effect of the fluorinated lead phosphate nonlinear optical frequency doubling crystal is about 1.8 times of that of KDP (potassium dihydrogen phosphate), and the ultraviolet cut-off edge is lower than 240 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonlinear optical frequency doubling crystals, and in particular relates to a compound lead fluorinated phosphate and a lead fluorinated phosphate nonlinear optical frequency doubling crystal, and a preparation method and application thereof. Background Art

[0002] Ultraviolet nonlinear optical frequency-doubling crystals can use their frequency conversion properties to convert near-infrared, visible and other band lasers into ultraviolet lasers, and have important application value in the fields of medicine, communications, scientific research, etc. As we all know, the currently practical short-wavelength nonlinear optical frequency-doubling crystal is KBe invented by Chinese scientists. 2 BO 3 F 2 (KBBF) crystal, BaB 2 O 4 (BBO) and LiB 3 O 5 (LBO), however, these crystals have defects such as difficulty in growing large-sized crystals and low birefringence, which limit their application to a certain extent. Therefore, it is of great significance and practical value to prepare and synthesize new short-wavelength nonlinear optical frequency-doubling crystal materials with excellent comprehensive performance. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a compound lead phosphate fluoride and a lead phosphate fluoride nonlinear optical frequency doubling crystal and a preparation method and use thereof. The chemical formula of the lead phosphate fluoride compound of the present invention is PbPO 3 F, molecular weight is 305.16, and the compound lead fluoride phosphate is prepared by solid phase reaction method or solution method.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A compound lead fluorinated phosphate with the chemical formula PbPO 3 F, molecular weight is 305.16.

[0006] The present invention also provides a method for preparing the compound lead fluorinated phosphate, which is prepared by a solid phase synthesis method or a solution method;

[0007] When the solid phase synthesis method is used for preparation, the steps are as follows: weigh a Pb-containing compound, a P-containing compound and a F-containing compound at a molar ratio of Pb:P:F=1:1:1, mix them evenly, raise the temperature to 300-600°C under vacuum or inert atmosphere, and keep the temperature constant for 24-120 hours to obtain the compound lead fluoride phosphate (PbPO 3 F);

[0008] When the solution method is used for preparation, the steps are as follows: weigh the Pb-containing compound, the P-containing compound and the F-containing compound in a molar ratio of Pb:P:F=1:1:1, mix them, add a solvent, place them in a dry, ventilated and light-proof place to volatilize the solvent for 24-120 hours, and then filter the filtrate to obtain the compound PbPO 3 F.

[0009] Preferably, in the preparation method of the compound lead fluorinated phosphate, when the solid phase synthesis method is adopted, the Pb-containing compound is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ; It should be noted that (NH 4 ) 2 PO 3 F contains both P and F. When (NH 4 ) 2 PO 3 When F is used as a raw material, it can be considered that compounds containing P and F are added at the same time, the same below.

[0010] When the solution method is used, the Pb-containing compound is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 , the solvent is deionized water, ethanol or acetone.

[0011] The present invention also provides a lead fluorinated phosphate nonlinear optical frequency doubling crystal, the chemical formula of which is PbPO 3 F, with a molecular weight of 305.16, belongs to the orthorhombic system, with a space group of Cc and unit cell parameters of α=90°,β=126.0920(10)°,γ=90°,the unit cell volume is

[0012] The present invention also provides a method for preparing the lead fluorinated phosphate nonlinear optical frequency doubling crystal, which grows the crystal by a melt method, a vacuum packaging method, a hydrothermal method or a room temperature solution volatilization method;

[0013] When the melt method is used to grow crystals, the following steps are included:

[0014] a. Pb-containing compound, P-containing compound and F-containing compound are weighed at a molar ratio of Pb:P:F=1:1:1, mixed evenly, heated to 300-600°C under vacuum or inert atmosphere, and kept at constant temperature for 24-120 hours to obtain PbPO 3 F polycrystalline powder;

[0015] b. PbPO obtained in step a 3 The F polycrystalline powder is heated to 500-900°C under vacuum or inert atmosphere and kept at this temperature for 10-120 hours to obtain a mixed melt;

[0016] c. Cool the mixed melt obtained in step b to 300°C at a rate of 0.1-2°C / h, and then cool to room temperature at a rate of 5-10°C / h to obtain PbPO 3 F seed crystal;

[0017] d. Growing crystals in the mixed melt by the Czochralski method: 3 The F seed crystal is fixed on the seed crystal rod, and PbPO is added from the top of the mixed melt prepared in step b. 3 The F seed crystal is applied with a crystal growth controller at a speed of 2-20 rpm, the seed crystal is pulled at a speed of 1-10 mm / day, and the temperature is lowered at a rate of 0.1-10°C / h. After the crystal growth stops, the lead fluorinated phosphate nonlinear optical frequency doubling crystal (PbPO 3 F nonlinear optical frequency doubling crystal);

[0018] Or use the pyrolysis method to grow crystals in the mixed melt: PbPO obtained in step c 3 The F seed crystal is fixed on the seed crystal rod, and PbPO is added from the top of the mixed melt prepared in step b. 3 The F seed crystal is cooled at a rate of 0.1-10°C / h to allow the crystal to grow for 5-15 hours, and the crystal is lifted but does not leave the liquid surface to continue growing, and this is repeated until the crystal growth stops, and the PbPO is obtained. 3 F nonlinear optical frequency doubling crystal;

[0019] Or use the crucible descent method to grow crystals in the mixed melt: PbPO obtained in step c 3 The F seed crystal is placed at the bottom of the crucible, and the PbPO prepared in step a is then 3F polycrystal is placed in a crucible, and then the crucible is sealed. The growth furnace temperature is raised to 550-750℃, and the temperature is kept constant for 10-120 hours. The crucible position is adjusted so that PbPO 3 The F seed crystal is slightly melted, and then the crucible is lowered at a speed of 1-10 mm / day. At the same time, the growth temperature is kept unchanged, or the temperature is lowered to 350°C at a cooling rate of 3°C / h. After the growth is completed, the temperature is quickly lowered to room temperature at a rate of 5-10°C / h to obtain the PbPO 3 F nonlinear optical frequency doubling crystal;

[0020] When the vacuum packaging method is used to grow crystals, the following steps are included:

[0021] a. Pb-containing compound, P-containing compound and F-containing compound are weighed at a molar ratio of Pb:P:F=1:1:1, mixed evenly, heated to 400-600°C under vacuum or inert atmosphere, and kept at constant temperature for 24-120 hours to obtain PbPO 3 F polycrystalline powder;

[0022] b. PbPO obtained in step a 3 The polycrystalline powder F and the co-solvent are mixed uniformly at a molar ratio of 0-1:0.1-6, placed in a quartz tube, sealed and placed in a muffle furnace, heated to 500-800°C, kept at a constant temperature for 5-120 hours, then cooled to 350°C at a rate of 0.1-3°C / h, and then cooled to room temperature at a rate of 5-10°C / h to obtain the PbPO 3 F nonlinear optical frequency doubling crystal;

[0023] When the hydrothermal method is used to grow crystals, the following steps are included:

[0024] a. Pb-containing compound, P-containing compound and F-containing compound are weighed at a molar ratio of Pb:P:F=1:1:1, mixed evenly, heated to 400-600°C under vacuum or inert atmosphere, and kept at constant temperature for 24-120 hours to obtain PbPO 3 F polycrystalline powder;

[0025] b. PbPO obtained in step a 3 The polycrystalline F powder was dissolved in deionized water, and the incompletely dissolved mixture was ultrasonically treated at 60°C to make it fully mixed and dissolved. 3 ·H 2 O adjusts the pH value to 2-6 to obtain a mixed solution;

[0026] c. Transfer the mixed solution obtained in step b into the inner lining of a high-pressure reactor, and tighten and seal the reactor;

[0027] d. Place the autoclave in a thermostat, raise the temperature to 100-300°C, keep the temperature constant for 5-8 days, and then cool it down to room temperature at a rate of 5-20°C / day to obtain the PbPO 3 F nonlinear optical frequency doubling crystal;

[0028] When the room temperature solution volatilization method is used to grow crystals, the following steps are included:

[0029] a. Weigh a Pb-containing compound, a P-containing compound and a F-containing compound in a molar ratio of Pb:P:F=1-2:1-3:1-2, mix them evenly, and dissolve them in a solution to obtain a mixed solution. Place the mixed solution in a glass container, seal it with weighing paper, place it in a static environment, pierce a plurality of small holes in the seal to adjust the evaporation rate of water in the aqueous solution, and leave it at room temperature for 5-20 days;

[0030] b. Waiting for the solution in step a to grow crystal particles at the bottom of the container until the size of the crystal particles no longer changes significantly, thereby obtaining seed crystals;

[0031] c. Select the one with better quality in step b (transparent area larger than 1*1cm 2 The seed crystal with a thickness greater than 0.5 cm is suspended in the mixed solution obtained in step b and allowed to stand for growth at room temperature for 10-30 days to obtain the PbPO 3 F nonlinear optical frequency doubling crystal.

[0032] Preferably, in the preparation method of the lead fluorinated phosphate nonlinear optical frequency doubling crystal, when the crystal is grown by melt method, the Pb-containing compound in step a is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ;

[0033] When the vacuum packaging method is used to grow crystals, the Pb-containing compound in step a is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3F, the F-containing compound is PbF 2 ; The cosolvent in step b is PbF 2 , H 3 PO 4 or P 2 O 5 ;

[0034] When the hydrothermal method is used to grow crystals, the Pb-containing compound in step a is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ;

[0035] When the room temperature solution volatilization method is used to grow crystals, the Pb-containing compound in step a is Pb(NO 3 ) 2 , PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ; The static environment described in step a refers to an environment without shaking, pollution, and air convection;

[0036] The present invention also provides the use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal in preparing the 1064nm fundamental frequency light output by the Nd:YAG laser for double-frequency and triple-frequency harmonic light output.

[0037] The present invention also provides the use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal in preparing a short-wavelength frequency doubling light output of 266nm.

[0038] The present invention also provides the use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal in preparing a frequency doubling generator, an up or down frequency converter or an optical parametric oscillator.

[0039] Compared with the prior art, the present invention has the following advantages and technical effects:

[0040] (1) In the present invention, by using a large crucible or container and extending the crystal growth period, a correspondingly large-sized PbPO can be obtained. 3 F nonlinear optical frequency doubling crystal, in which PbPO 3 During the growth process of F nonlinear optical frequency doubling crystal, the crystal is easy to grow, transparent and without wrapping, and has the advantages of fast growth speed, low cost, and easy acquisition of large-size crystals.

[0041] (2) The preparation method of the present invention can obtain large-sized PbPO 3 F nonlinear optical frequency doubling crystal, according to the crystal crystallographic data, the crystal blank is oriented, the crystal is cut according to the required angle, thickness and cross-sectional size, and the light-transmitting surface of the crystal is polished, and it can be used as a nonlinear optical device. 3 F nonlinear optical frequency doubling crystal has a light transmission band of about 240nm, and has the advantages of stable physical and chemical properties (the crystal quality and mass do not change significantly within 2 months exposed to air at room temperature) and not easy to deliquesce (no deliquesce occurs within 2 months exposed to air at room temperature). BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0043] Figure 1 The compound PbPO in Example 1 of the present invention 3 Powder XRD spectrum of F;

[0044] Figure 2 is PbPO in Example 6 of the present invention 3 F. Unit cell structure diagram of nonlinear optical frequency doubling crystal;

[0045] Figure 3 To use the PbPO of the present invention 3 The working principle diagram of the nonlinear optical device made of F nonlinear optical frequency doubling crystal, where 1 is the laser, 2 is the emitted light beam, and 3 is PbPO 3 F is a nonlinear optical frequency doubling crystal, 4 is an output beam, and 5 is a filter. DETAILED DESCRIPTION

[0046] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0047] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0048] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0049] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0050] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0051] In the present invention, unless otherwise specified, room temperature is 25±2°C.

[0052] All raw materials and equipment used in the embodiments of the present invention are commercially available.

[0053] The embodiment of the present invention provides a compound lead fluorinated phosphate, the chemical formula of which is PbPO 3 F, molecular weight is 305.16.

[0054] The embodiment of the present invention also provides a method for preparing the compound lead fluorinated phosphate, which is prepared by a solid phase synthesis method or a solution method;

[0055] When the solid phase synthesis method is used for preparation, the steps are as follows: weigh a Pb-containing compound, a P-containing compound and a F-containing compound at a molar ratio of Pb:P:F=1:1:1, mix them evenly, put them into a platinum crucible, place them in a muffle furnace under vacuum or inert atmosphere, heat them to 300-600°C, and keep the temperature constant for 24-120 hours to obtain the compound lead fluoride phosphate (PbPO 3 F), the Pb-containing compound is PbO, PbF2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ;

[0056] When the solution method is used for preparation, the steps are as follows: weigh the Pb-containing compound, the P-containing compound and the F-containing compound in a molar ratio of Pb:P:F=1:1:1, mix them, add a solvent, place them in a dry, ventilated and light-proof place to volatilize the solvent for 24-120 hours, and then filter the filtrate to obtain the compound PbPO 3 F, the Pb-containing compound is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 , the solvent is deionized water, ethanol or acetone.

[0057] The embodiment of the present invention also provides a lead fluorinated phosphate nonlinear optical frequency doubling crystal, the chemical formula of the crystal is PbPO 3 F, with a molecular weight of 305.16, belongs to the orthorhombic system, with a space group of Cc and unit cell parameters of α=90°,β=126.0920(10)°,γ=90°,the unit cell volume is

[0058] In an embodiment of the present invention, a method for preparing the lead fluorinated phosphate nonlinear optical frequency doubling crystal is also provided, wherein the crystal is grown by a melt method, a vacuum packaging method, a hydrothermal method or a room temperature solution volatilization method;

[0059] When the melt method is used to grow crystals, the following steps are included:

[0060] a. Pb-containing compound, P-containing compound and F-containing compound are weighed at a molar ratio of Pb:P:F=1:1:1, mixed evenly, put into a platinum crucible, placed in a muffle furnace under vacuum or inert atmosphere, heated to 300-600°C, and kept at this temperature for 24-120 hours to obtain PbPO3 F polycrystalline powder, the Pb-containing compound is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ;

[0061] b. PbPO obtained in step a 3 The F polycrystalline powder is loaded into a platinum crucible, placed in a muffle furnace under vacuum or inert atmosphere, heated to 500-900° C., and kept at this temperature for 10-120 hours to obtain a mixed melt;

[0062] c. Cool the mixed melt obtained in step b to 300°C at a rate of 0.1-2°C / h, and then cool to room temperature at a rate of 5-10°C / h to obtain PbPO 3 F seed crystal;

[0063] d. Growing crystals in the mixed melt by the Czochralski method: 3 The F seed crystal is fixed on the seed crystal rod, and PbPO is added from the top of the mixed melt prepared in step b. 3 The F seed crystal is applied with a crystal growth controller at a speed of 2-20 rpm, the seed crystal is pulled at a speed of 1-10 mm / day, and the temperature is lowered at a rate of 0.1-10°C / h. After the crystal growth stops, the lead fluorinated phosphate nonlinear optical frequency doubling crystal (PbPO 3 F nonlinear optical frequency doubling crystal);

[0064] Or use the pyrolysis method to grow crystals in the mixed melt: PbPO obtained in step c 3 The F seed crystal is fixed on the seed crystal rod, and PbPO is added from the top of the mixed melt prepared in step b. 3 The F seed crystal is cooled at a rate of 0.1-10°C / h to allow the crystal to grow for 5-15 hours, and the crystal is lifted but does not leave the liquid surface to continue growing, and this is repeated until the crystal growth stops, and the PbPO is obtained. 3 F nonlinear optical frequency doubling crystal;

[0065] Or use the crucible descent method to grow crystals in the mixed melt: PbPO obtained in step c 3 The F seed crystal is placed at the bottom of the crucible, and the PbPO prepared in step a is then 3F polycrystal is placed in a crucible, and then the crucible is sealed. The growth furnace temperature is raised to 550-750℃, and the temperature is kept constant for 10-120 hours. The crucible position is adjusted so that PbPO 3 The F seed crystal is slightly melted, and then the crucible is lowered at a speed of 1-10 mm / day. At the same time, the growth temperature is kept unchanged, or the temperature is lowered to 350°C at a cooling rate of 3°C / h. After the growth is completed, the temperature is quickly lowered to room temperature at a rate of 5-10°C / h to obtain the PbPO 3 F nonlinear optical frequency doubling crystal;

[0066] When the vacuum packaging method is used to grow crystals, the following steps are included:

[0067] a. Pb-containing compound, P-containing compound and F-containing compound are weighed at a molar ratio of Pb:P:F=1:1:1, mixed evenly, put into a platinum crucible, placed in a muffle furnace under vacuum or inert atmosphere, heated to 400-600°C, and kept at this temperature for 24-120 hours to obtain PbPO 3 F polycrystalline powder, the Pb-containing compound is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ;

[0068] b. PbPO obtained in step a 3 The molar ratio of F polycrystalline powder to solvent is 0-1:0.1-6 (PbPO 3 The molar number of the polycrystalline powder F is not 0) is mixed evenly, put into a quartz tube, sealed and placed in a muffle furnace, heated to 500-800°C, kept at a constant temperature for 5-120 hours, then cooled to 350°C at a rate of 0.1-3°C / h, and then cooled to room temperature at a rate of 5-10°C / h to obtain the PbPO 3 F nonlinear optical frequency doubling crystal, the cosolvent is PbF 2 , H 3 PO 4 or P 2 O 5 ;

[0069] When the hydrothermal method is used to grow crystals, the following steps are included:

[0070] a. Pb-containing compound, P-containing compound and F-containing compound are weighed at a molar ratio of Pb:P:F=1:1:1, mixed evenly, heated to 400-600°C under vacuum or inert atmosphere, and kept at constant temperature for 24-120 hours to obtain PbPO 3 F polycrystalline powder, the Pb-containing compound is PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P 2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ;

[0071] b. PbPO obtained in step a 3 The polycrystalline F powder was dissolved in deionized water, and the incompletely dissolved mixture was ultrasonically treated at 60°C to make it fully mixed and dissolved. 3 ·H 2 O adjusts the pH value to 2-6 to obtain a mixed solution;

[0072] c. Transfer the mixed solution obtained in step b into the inner liner of the autoclave, and tighten and seal the autoclave;

[0073] d. Place the autoclave in a thermostat, raise the temperature to 100-300°C, keep the temperature constant for 5-8 days, and then cool it down to room temperature at a rate of 5-20°C / day to obtain the PbPO 3 F nonlinear optical frequency doubling crystal;

[0074] When the room temperature solution volatilization method is used to grow crystals, the following steps are included:

[0075] a. Pb-containing compound, P-containing compound and F-containing compound are weighed in a molar ratio of Pb:P:F=1-2:1-3:1-2, mixed evenly, and dissolved in a solution to obtain a mixed solution. The mixed solution is placed in a clean glass container, sealed with weighing paper, and placed in a static environment without shaking, pollution, and air convection. A plurality of small holes are punched in the seal to adjust the evaporation rate of water in the aqueous solution, and the mixture is left standing at room temperature for 5-20 days. The Pb-containing compound is Pb(NO 3 ) 2 , PbO, PbF 2 or Pb(NO 3 ) 2 , the P-containing compound is H 3 PO 4 , P2 O 5 or (NH 4 ) 2 PO 3 F, the F-containing compound is PbF 2 ;

[0076] b. Waiting for the solution in step a to grow crystal particles at the bottom of the container until the size of the crystal particles no longer changes significantly, thereby obtaining seed crystals;

[0077] c. Select the one with better quality in step b (transparent area larger than 1*1cm 2 , with a thickness greater than 0.5 cm), suspending the seed crystal in the mixed solution obtained in step b, and letting it stand and grow at room temperature for 10-30 days to obtain the PbPO 3 F nonlinear optical frequency doubling crystal,

[0078] The present invention also provides the use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal in preparing the 1064nm fundamental frequency light output by the Nd:YAG laser for double-frequency and triple-frequency harmonic light output.

[0079] The present invention also provides the use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal in preparing a short-wavelength frequency doubling light output of 266nm.

[0080] The present invention also provides the use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal in preparing a frequency doubling generator, an up or down frequency converter or an optical parametric oscillator.

[0081] In the preparation method of the fluorinated lead phosphate nonlinear optical frequency doubling crystal of the embodiment of the present invention, the container used in the preparation process is a platinum crucible, an iridium crucible, a ceramic crucible, a quartz tube, a conical flask, a beaker, and a hydrothermal kettle lined with a polytetrafluoroethylene liner or a stainless steel liner equipped with a platinum sleeve. When the container is a quartz tube, it needs to be evacuated before sealing to avoid the volatilization of the raw materials during the reaction and the explosion of the quartz tube. When the container is a conical flask or a beaker, the container must be cleaned with acid first, then rinsed with deionized water, and dried.

[0082] The technical solution of the present invention is further illustrated by the following embodiments.

[0083] Example 1

[0084] According to the reaction formula: Pb(NO 3 ) 2 +(NH 4 ) 2 PO 3 F→PbPO 3 F+2NH 4 NO 3 , the compound PbPO was synthesized by solid phase reaction method3 F:

[0085] Pb(NO 3 ) 2 and (NH 4 ) 2 PO 3 F were mixed evenly in a molar ratio of 1:1, loaded into a platinum crucible, placed in a muffle furnace, and heated to 450°C under vacuum conditions and kept at this temperature for 48 hours to obtain the compound PbPO 3 F polycrystalline powder.

[0086] The compound PbPO in Example 1 of the present invention 3 The powder XRD spectrum of F is shown in Figure 1 .

[0087] Example 2

[0088] According to the reaction formula: PbO+PbF 2 +2H 3 PO 4 →2PbPO 3 F+3H 2 O Synthesis of compound PbPO by solid phase reaction method 3 F:

[0089] PbO, H 3 PO 4 and PbF 2 The mixture was mixed evenly in a molar ratio of 1:2:1, placed in a platinum crucible, placed in a muffle furnace, heated to 300°C under an inert atmosphere, and kept at this temperature for 120 hours to obtain the compound PbPO 3 F polycrystalline powder.

[0090] Example 3

[0091] According to the reaction formula: PbO+PbF 2 +P 2 O 5 →2PbPO 3 F Synthesis of compound PbPO by solid phase reaction method 3 F:

[0092] PbO, PbF 2 and P 2 O 5 The mixture was mixed evenly in a molar ratio of 1:1, placed in a platinum crucible, placed in a muffle furnace, heated to 600°C under an inert atmosphere, and kept at this temperature for 24 hours to obtain the compound PbPO 3 F polycrystalline powder.

[0093] Example 4

[0094] According to the reaction formula: Pb(NO3 ) 2 +(NH 4 ) 2 PO 3 F→PbPO 3 F+2NH 4 NO 3 , the compound PbPO was synthesized by solution method 3 F:

[0095] Pb(NO 3 ) 2 and (NH 4 ) 2 PO 3 F was mixed evenly in a molar ratio of 1:1, and deionized water was added to prepare a saturated solution. The solution was placed in a dry, ventilated and dark place to evaporate the solvent for 48 hours, and then the filtrate was filtered to obtain the compound PbPO 3 F polycrystalline powder.

[0096] Example 5

[0097] According to the reaction formula: PbO+PbF 2 +2H 3 PO 4 →2PbPO 3 F+3H 2 O Synthesis of compound PbPO by solution method 3 F:

[0098] PbO, H 3 PO 4 and PbF 2 Mix evenly in a molar ratio of 1:2:1, add deionized water with 2 times the amount of phosphoric acid, place in a dry, ventilated and dark place to evaporate the solvent for 120 hours, and then filter the filtrate to obtain the compound PbPO 3 F polycrystalline powder.

[0099] Example 6

[0100] Melt-grown PbPO 3 F nonlinear optical frequency doubling crystal:

[0101] a. Compound PbPO prepared in Example 1 3 The F polycrystalline powder is loaded into a platinum crucible, placed in a muffle furnace, and heated to 600°C under vacuum conditions and kept at this temperature for 80 hours to obtain a mixed melt;

[0102] b. The mixed melt was slowly cooled to 300°C at a rate of 0.1°C / h, and then rapidly cooled to room temperature at a rate of 5°C / h to obtain PbPO 3 F seed crystal;

[0103] c. Use the Czochralski method to grow crystals in the mixed melt: 3 The F seed crystal is fixed on the seed crystal rod, and PbPO is lowered from the top of the mixed melt. 3 The F seed crystal is rotated at 2 rpm by a crystal growth controller, the seed crystal is pulled at a speed of 1 mm / day, and the temperature is lowered at a rate of 0.1 °C / h. After the crystal growth stops, a PbPO with a size of 18 mm × 15 mm × 10 mm is obtained. 3 F nonlinear optical frequency doubling crystal.

[0104] In the embodiment of the present invention, PbPO 3 The unit cell structure of the F nonlinear optical frequency doubling crystal is shown in Figure 2 , we know that the chemical formula of the crystal is PbPO 3 F, with a molecular weight of 305.16, belongs to the orthorhombic system, with a space group of Cc and unit cell parameters of α=90°,β=126.0920(10)°,γ=90°,the unit cell volume is

[0105] Example 7

[0106] Melt-grown PbPO 3 F nonlinear optical frequency doubling crystal:

[0107] a. Compound PbPO prepared in Example 5 3 The F polycrystalline powder is loaded into a platinum crucible, placed in a muffle furnace, and heated to 600°C in an inert atmosphere and kept at this temperature for 10 hours to obtain a mixed melt;

[0108] b. The mixed melt was slowly cooled to 300°C at a rate of 1°C / h, and then rapidly cooled to room temperature at a rate of 8°C / h to obtain PbPO 3 F seed crystal;

[0109] c. Growing crystals from the mixed melt by the Czochralski method: 3 The F seed crystal is fixed on the seed crystal rod, and PbPO is lowered from the top of the mixed melt. 3 The F seed crystal is rotated at 10 rpm by a crystal growth controller, the seed crystal is pulled at a speed of 5 mm / day, and the temperature is lowered at a rate of 5 °C / h. After the crystal growth stops, a PbPO with a size of 15 mm×10 mm×10 mm is obtained. 3 F nonlinear optical frequency doubling crystal.

[0110] Example 8

[0111] Melt-grown PbPO 3F nonlinear optical frequency doubling crystal:

[0112] a. Compound PbPO prepared in Example 4 3 The F polycrystalline powder is loaded into a platinum crucible, placed in a muffle furnace under an inert atmosphere, heated to 600°C, and kept at this temperature for 50 hours to obtain a mixed melt;

[0113] b. The obtained mixed melt was slowly cooled to 300°C at a rate of 1°C / h, and then rapidly cooled to room temperature at a rate of 8°C / h to obtain PbPO 3 F seed crystal;

[0114] c. Use the pyrolysis method to grow crystals in the mixed melt: the obtained PbPO 3 The F seed crystal is fixed on the seed crystal rod, and PbPO is lowered from the top of the mixed melt. 3 The F seed crystal was cooled at a rate of 0.1°C / h to allow the crystal to grow for 5 hours. The crystal was slowly lifted but not out of the liquid surface to continue growing. This process was repeated until the crystal growth stopped, and a PbPO with a size of 20 mm × 15 mm × 12 mm was obtained. 3 F nonlinear optical frequency doubling crystal.

[0115] Example 9

[0116] Melt-grown PbPO 3 F nonlinear optical frequency doubling crystal:

[0117] a. Compound PbPO prepared in Example 6 3 The F polycrystalline powder is loaded into a platinum crucible, placed in a muffle furnace under vacuum conditions, heated to 800°C, and kept at this temperature for 100 hours to obtain a mixed melt;

[0118] b. The obtained mixed melt was slowly cooled to 300°C at a rate of 2°C / h, and then rapidly cooled to room temperature at a rate of 10°C / h to obtain PbPO 3 F seed crystal;

[0119] c. Use the crucible descent method to grow crystals in the mixed melt: 3 The F seed crystal was placed at the bottom of the platinum crucible, and the compound PbPO prepared in Example 6 was added. 3 The F polycrystalline powder was placed in a platinum crucible, which was then sealed. The temperature of the growth furnace was raised to 750°C and kept constant for 10 hours. The position of the platinum crucible was adjusted to allow the seed crystal to melt slightly. The crucible was then lowered at a rate of 1 mm / day and cooled to 350°C at a rate of 3°C / h. After the growth was completed, the temperature was quickly cooled to room temperature at a rate of 10°C / h to obtain a PbPO with a size of 20 mm×16 mm×13 mm. 3 F nonlinear optical frequency doubling crystal.

[0120] Example 10

[0121] Growth of PbPO by vacuum encapsulation method 3 F nonlinear optical frequency doubling crystal:

[0122] The compound PbPO prepared in Example 2 3 F polycrystalline powder and solvent PbF 2 The molar ratio was 1:3 and the quartz tube was evacuated to a vacuum degree of 1×10 -3 Pa, sealed at high temperature, placed in a muffle furnace, heated to 650 ° C, kept constant for 5 hours, then cooled to 350 ° C at a rate of 0.1 ° C / h, and then quickly cooled to room temperature at a rate of 8 ° C / h, to obtain a PbPO with a size of 4 mm × 4 mm × 2 mm 3 F nonlinear optical frequency doubling crystal.

[0123] Embodiment 11

[0124] Hydrothermal method was used to grow lead fluorinated phosphate nonlinear optical frequency doubling crystals:

[0125] a. Compound PbPO prepared in Example 3 3 The polycrystalline powder of F was dissolved in deionized water, and the incompletely dissolved mixture was subjected to ultrasonic treatment at 60°C to allow it to be fully mixed and dissolved. 3 ·H 2 O adjusted the pH value to 3 to obtain a mixed solution;

[0126] b. Transfer the obtained mixed solution into the liner of a clean, pollution-free autoclave with a volume of 100 mL, and tighten and seal the autoclave;

[0127] c. Place the autoclave in a thermostat, raise the temperature to 150°C, keep the temperature constant for 8 days, and then cool it down to room temperature at a rate of 5°C / day to obtain PbPO with a size of 5mm×3mm×2mm. 3 F nonlinear optical frequency doubling crystal.

[0128] Example 12

[0129] Growing lead fluorinated phosphate nonlinear optical frequency doubling crystals using room temperature solution method:

[0130] a. Compound PbPO prepared in Example 1 3 The F polycrystalline powder was placed in a clean glass container, 20 mL of deionized water was added, and then ultrasonic treatment was performed to fully mix and dissolve. 3 ·H 2 O adjusted the solution pH to 3, and filtered with filter paper to obtain a mixed solution;

[0131] b. Place the obtained mixed solution in a clean conical flask, seal it with weighing paper, place it in a static environment without shaking, pollution, or air convection, pierce several small holes in the seal to adjust the evaporation rate of water in the aqueous solution, and leave it at room temperature for 5 days;

[0132] c. Wait for the solution to grow crystal particles at the bottom of the container until the size of the crystal particles no longer changes significantly, thereby obtaining seed crystals;

[0133] d. Select a seed crystal with good quality, suspend it in the mixed solution obtained in step a, and let it stand at room temperature for 30 days to obtain a PbPO with a size of 10 mm × 8 mm × 6 mm. 3 F nonlinear optical frequency doubling crystal.

[0134] Embodiment 13

[0135] Same as Example 12, except that the growth time in step d is 10 days, and the PbPO with a size of 15 mm×10 mm×10 mm is obtained. 3 F nonlinear optical frequency doubling crystal.

[0136] Embodiment 14

[0137] Hydrothermal method was used to grow lead fluorinated phosphate nonlinear optical frequency doubling crystals:

[0138] a. Compound PbPO prepared in Example 4 3 The polycrystalline powder of F was dissolved in deionized water, and the incompletely dissolved mixture was subjected to ultrasonic treatment at 60°C to allow it to be fully mixed and dissolved. 3 ·H 2 O adjusted the pH value to 6 to obtain a mixed solution;

[0139] b. Transfer the obtained mixed solution into the liner of a clean, pollution-free autoclave with a volume of 100 mL, and tighten and seal the autoclave;

[0140] c. Place the autoclave in a thermostat, raise the temperature to 300°C, keep the temperature constant for 5 days, and then cool it down to room temperature at a rate of 20°C / day to obtain PbPO with a size of 18mm×15mm×12mm. 3 F nonlinear optical frequency doubling crystal.

[0141] Embodiment 15

[0142] Growth of PbPO by vacuum encapsulation method 3 F nonlinear optical frequency doubling crystal:

[0143] The compound PbPO prepared in Example 2 3 F polycrystalline powder and solvent H3 PO 4 The molar ratio was 1:6 and the quartz tube was evacuated to a vacuum degree of 1×10 -3 Pa, sealed at high temperature, placed in a muffle furnace, heated to 800 ° C, kept constant for 40 hours, then cooled to 350 ° C at a rate of 3 ° C / h, and then quickly cooled to room temperature at a rate of 5 ° C / h, to obtain a PbPO with a size of 10 mm × 10 mm × 5 mm 3 F nonlinear optical frequency doubling crystal.

[0144] Example 16

[0145] Growth of PbPO by vacuum encapsulation method 3 F nonlinear optical frequency doubling crystal:

[0146] The compound PbPO prepared in Example 3 3 F polycrystalline powder and solvent P 2 O 5 The molar ratio was 1:0.1 and the quartz tube was evacuated to a vacuum degree of 1×10 -3 Pa, sealed at high temperature, placed in a muffle furnace, heated to 500 ° C, kept at this temperature for 120 hours, then cooled to 350 ° C at a rate of 0.1 ° C / h, and then quickly cooled to room temperature at a rate of 10 ° C / h, thus obtaining a PbPO with a size of 10 mm × 10 mm × 8 mm. 3 F nonlinear optical frequency doubling crystal.

[0147] Embodiment 17

[0148] Melt-grown PbPO 3 F nonlinear optical frequency doubling crystal:

[0149] a. Compound PbPO prepared in Example 6 3 The F polycrystalline powder is loaded into a platinum crucible, placed in a muffle furnace under an inert atmosphere, heated to 500°C, and kept at this temperature for 10 hours to obtain a mixed melt;

[0150] b. The obtained mixed melt was slowly cooled to 300°C at a rate of 0.1°C / h, and then rapidly cooled to room temperature at a rate of 5°C / h to obtain PbPO 3 F seed crystal;

[0151] c. Use the crucible descent method to grow crystals in the mixed melt: 3 The F seed crystal was placed at the bottom of the platinum crucible, and the compound PbPO prepared in Example 6 was added. 3The polycrystalline powder F was placed in a platinum crucible, which was then sealed. The temperature of the growth furnace was raised to 550°C and kept constant for 120 hours. The position of the platinum crucible was adjusted to allow the seed crystal to melt slightly. The crucible was then lowered at a rate of 10 mm / day to keep the temperature constant. After the growth was completed, the crucible was quickly lowered to room temperature at a rate of 5°C / h to obtain a PbPO with a size of 10 mm×10 mm×5 mm. 3 F nonlinear optical frequency doubling crystal.

[0152] Embodiment 18

[0153] Melt-grown PbPO 3 F nonlinear optical frequency doubling crystal:

[0154] a. Compound PbPO prepared in Example 4 3 The F polycrystalline powder is loaded into a platinum crucible, placed in a muffle furnace under an inert atmosphere, heated to 800°C, and kept at this temperature for 100 hours to obtain a mixed melt;

[0155] b. The obtained mixed melt was slowly cooled to 300°C at a rate of 1°C / h, and then rapidly cooled to room temperature at a rate of 6°C / h to obtain PbPO 3 F seed crystal;

[0156] c. Use the pyrolysis method to grow crystals in the mixed melt: the obtained PbPO 3 The F seed crystal is fixed on the seed crystal rod, and PbPO is lowered from the top of the mixed melt. 3 The F seed crystal was cooled at a rate of 10°C / h, and the crystal was allowed to grow for 5 hours. The crystal was slowly lifted but not out of the liquid surface, and continued to grow. This process was repeated until the crystal growth stopped, and a PbPO with a size of 15 mm × 12 mm × 10 mm was obtained. 3 F nonlinear optical frequency doubling crystal.

[0157] Test Example 1

[0158] Figure 3 To use the PbPO of the present invention 3 Working principle diagram of nonlinear optical device made of nonlinear optical frequency doubling crystal (PbPO prepared in Example 7 3 F nonlinear optical frequency doubling crystal as an example), where 1 is the laser, 2 is the emitted light beam, and 3 is PbPO 3 F is a nonlinear optical frequency doubling crystal, 4 is an output beam, and 5 is a filter. 3 F nonlinear optical frequency doubling crystal is processed according to the matching direction. Figure 3 As shown, the PbPO 3At the position of the nonlinear optical frequency doubling crystal 3, at room temperature, a Q-switched Nd:YAG laser is used as the light source, and the incident wavelength is 1064nm. The infrared beam 2 with a wavelength of 1064nm emitted by the Q-switched Nd:YAG laser 1 is injected into the PbPO 3 F nonlinear optical frequency doubling crystal 3, produces green frequency doubling light 4 with a wavelength of 532nm, and the output intensity after passing through filter 5 is about the same as KH under the same conditions 2 PO 4 The ultraviolet cutoff edge is lower than 240nm, and it can be used as a short-wavelength nonlinear optical frequency doubling in all-solid-state lasers.

[0159] Test Example 2

[0160] Same test process as test example 1 ( Figure 3 ), a KDP filter is added at the exit of the Q-Nd:YAG laser, and a green laser with a wavelength of 532nm is incident on the PbPO 3 F nonlinear optical frequency doubling crystal 3 generates frequency doubling light 4 with a wavelength of 266nm, and the output intensity after passing through filter 5 is about the same as BaB under the same conditions 2 O 4 It is 0.5 times of that of the laser and can be used as a nonlinear optical frequency doubling device in the short wavelength and ultraviolet region in all-solid-state lasers.

[0161] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A compound lead fluorinated phosphate, characterized in that The chemical formula is PbPO3F and the molecular weight is 305.

16.

2. A method for preparing the compound lead fluorinated phosphate according to claim 1, characterized in that: Prepared by solid phase synthesis or solution method; When the solid phase synthesis method is used for preparation, the steps are as follows: weighing a Pb-containing compound, a P-containing compound and a F-containing compound at a molar ratio of Pb:P:F=1:1:1, mixing them uniformly, heating to 300-600°C under vacuum or inert atmosphere, and keeping the temperature constant for 24-120 hours to obtain a compound of lead fluoride phosphate; When the solution method is used for preparation, the steps are as follows: weighing a Pb-containing compound, a P-containing compound and a F-containing compound in a molar ratio of Pb:P:F=1:1:1, adding a solvent, placing in a dry, ventilated and light-proof place to volatilize the solvent for 24-120 hours, and then filtering the filtrate to obtain the compound lead fluoride phosphate.

3. The method for preparing the compound lead fluorinated phosphate according to claim 2, characterized in that: When the solid phase synthesis method is adopted, the Pb-containing compound is PbO, PbF2 or Pb(NO3)2, the P-containing compound is H3PO4, P2O5 or (NH4)2PO3F, and the F-containing compound is PbF2; When the solution method is adopted, the Pb-containing compound is PbO, PbF2 or Pb(NO3)2, the P-containing compound is H3PO4, P2O5 or (NH4)2PO3F, the F-containing compound is PbF2, and the solvent is deionized water, ethanol or acetone.

4. A lead fluorinated phosphate nonlinear optical frequency doubling crystal, characterized in that: The chemical formula of the crystal is PbPO3F, the molecular weight is 305.16, it belongs to the orthorhombic system, the space group is Cc, and the unit cell parameters are α=90°,β=126.0920(10)°,γ=90°,the unit cell volume is 5. A method for preparing the lead fluorinated phosphate nonlinear optical frequency doubling crystal according to claim 4, characterized in that: Growing crystals by melt method, vacuum encapsulation method, hydrothermal method or room temperature solution evaporation method; When the melt method is used to grow crystals, the following steps are included: a. Weigh a Pb-containing compound, a P-containing compound and a F-containing compound at a molar ratio of Pb:P:F=1:1:1, mix them evenly, raise the temperature to 300-600°C under vacuum or inert atmosphere, and keep the temperature constant for 24-120 hours to obtain PbPO3F polycrystalline powder; b. The PbPO3F polycrystalline powder obtained in step a is heated to 500-900° C. under vacuum or inert atmosphere and kept at this temperature for 10-120 hours to obtain a mixed melt; c. Cooling the mixed melt obtained in step b to 300° C. at a rate of 0.1-2° C. / h, and then cooling to room temperature at a rate of 5-10° C. / h to obtain PbPO3F seed crystals; d. Growing crystals in the mixed melt by the Czochralski method: fixing the PbPO3F seed crystal obtained in step c on a seed crystal rod, placing the PbPO3F seed crystal from the top of the mixed melt obtained in step b, applying a crystal rotation of 2-20 rpm through a crystal growth controller, pulling the seed crystal at a speed of 1-10 mm / day, and cooling at a rate of 0.1-10°C / h. After the crystal growth stops, the lead fluorinated phosphate nonlinear optical frequency doubling crystal is obtained; Or the crystal is grown in the mixed melt by the pyrolysis method: the PbPO3F seed crystal obtained in step c is fixed on the seed crystal rod, the PbPO3F seed crystal is placed from the top of the mixed melt obtained in step b, the temperature is lowered at a rate of 0.1-10°C / h, the crystal is grown for 5-15 hours, the crystal is lifted but does not leave the liquid surface to continue growing, and this is repeated until the crystal growth stops, and the lead fluorinated phosphate nonlinear optical frequency doubling crystal is obtained; Or a crystal is grown in a mixed melt by a crucible lowering method: the PbPO3F seed crystal obtained in step c is placed at the bottom of the crucible, and the PbPO3F polycrystal prepared in step a is placed in the crucible, and then the crucible is sealed, the temperature of the growth furnace is raised to 550-750°C, and the temperature is kept constant for 10-120 hours, the position of the crucible is adjusted to make the PbPO3F seed crystal slightly melted, and then the crucible is lowered at a rate of 1-10 mm / day, and at the same time, the growth temperature is kept unchanged, or the temperature is lowered to 350°C at a cooling rate of 3°C / h, and after the growth is completed, the temperature is quickly lowered to room temperature at a rate of 5-10°C / h, so as to obtain the lead fluorinated phosphate nonlinear optical frequency doubling crystal; When the vacuum packaging method is used to grow crystals, the following steps are included: a. Weigh a Pb-containing compound, a P-containing compound and a F-containing compound at a molar ratio of Pb:P:F=1:1:1, mix them evenly, raise the temperature to 400-600°C under vacuum or inert atmosphere, and keep the temperature constant for 24-120 hours to obtain PbPO3F polycrystalline powder; b. The PbPO3F polycrystalline powder obtained in step a is mixed evenly with a co-solvent at a molar ratio of 0-1:0.1-6, and the mixture is placed in a quartz tube, sealed and placed in a muffle furnace, heated to 500-800°C, kept at a constant temperature for 5-120 hours, then cooled to 350°C at a rate of 0.1-3°C / h, and then cooled to room temperature at a rate of 5-10°C / h, to obtain the lead fluorinated phosphate nonlinear optical frequency doubling crystal; When the hydrothermal method is used to grow crystals, the following steps are included: a. Weigh a Pb-containing compound, a P-containing compound and a F-containing compound at a molar ratio of Pb:P:F=1:1:1, mix them evenly, raise the temperature to 400-600°C under vacuum or inert atmosphere, and keep the temperature constant for 24-120 hours to obtain PbPO3F polycrystalline powder; b. The PbPO3F polycrystalline powder obtained in step a is dissolved in deionized water, and the incompletely dissolved mixture is subjected to ultrasonic treatment at a temperature of 60° C. to allow the mixture to be fully mixed and dissolved, and the pH value is adjusted to 2-6 with HF and NH3·H2O to obtain a mixed solution; c. Transfer the mixed solution obtained in step b into the inner lining of a high-pressure reactor, and tighten and seal the reactor; d. placing the high-pressure reactor in a constant temperature box, raising the temperature to 100-300° C., maintaining the temperature for 5-8 days, and then cooling the temperature down to room temperature at a rate of 5-20° C. / day, thereby obtaining the lead fluorinated phosphate nonlinear optical frequency doubling crystal; When the room temperature solution volatilization method is used to grow crystals, the following steps are included: a. Weigh a Pb-containing compound, a P-containing compound and a F-containing compound in a molar ratio of Pb:P:F=1-2:1-3:1-2, mix them evenly, and dissolve them in a solution to obtain a mixed solution. Place the mixed solution in a glass container, seal it with weighing paper, place it in a static environment, pierce a plurality of small holes in the seal to adjust the evaporation rate of water in the aqueous solution, and leave it at room temperature for 5-20 days; b. Waiting for the solution in step a to grow crystal particles at the bottom of the container until the size of the crystal particles no longer changes significantly, thereby obtaining seed crystals; c. Select the seed crystal with better quality in step b, suspend it in the mixed solution prepared in step b, and let it stand and grow at room temperature for 10-30 days to obtain the lead fluorinated phosphate nonlinear optical frequency doubling crystal.

6. The method for preparing the lead fluorinated phosphate nonlinear optical frequency doubling crystal according to claim 5, characterized in that: When the crystal is grown by the melt method, the Pb-containing compound in step a is PbO, PbF2 or Pb(NO3)2, the P-containing compound is H3PO4, P2O5 or (NH4)2PO3F, and the F-containing compound is PbF2; When the vacuum packaging method is used to grow the crystal, the Pb-containing compound in step a is PbO, PbF2 or Pb(NO3)2, the P-containing compound is H3PO4, P2O5 or (NH4)2PO3F, and the F-containing compound is PbF2; the cosolvent in step b is PbF2, H3PO4 or P2O5; When the crystal is grown by hydrothermal method, the Pb-containing compound in step a is PbO, PbF2 or Pb(NO3)2, the P-containing compound is H3PO4, P2O5 or (NH4)2PO3F, and the F-containing compound is PbF2; When the room temperature solution volatilization method is used to grow crystals, the Pb-containing compound in step a is Pb(NO3)2, PbO, PbF2 or Pb(NO3)2, the P-containing compound is H3PO4, P2O5 or (NH4)2PO3F, and the F-containing compound is PbF2; the static environment in step a refers to an environment without shaking, pollution, and air convection.

7. Use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal according to claim 4 in preparing the 1064nm fundamental frequency light output by Nd:YAG laser for double-frequency and triple-frequency harmonic light output.

8. Use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal according to claim 4 in the preparation of a short-wavelength frequency doubling light output of 266 nm.

9. Use of the lead fluorinated phosphate nonlinear optical frequency doubling crystal according to claim 4 in preparing a frequency doubling generator, an up or down frequency converter or an optical parametric oscillator.

Citation Information

Patent Citations

  • Ammonium monofluorophosphate nonlinear optical crystal as well as preparation method and use

    CN108330539A

  • Compound lead fluoroborate, lead fluoroborate nonlinear optical crystal, preparation method and application

    CN110921676A

  • Method of producing lead fluorophosphate

    SU710929A1

Cited By

  • Guanidine nitrate nonlinear optical crystal as well as preparation method and application thereof

    CN120193338A