Composite nanofiber membrane with aperture hierarchical structure as well as preparation method and application of composite nanofiber membrane
Through the composite nanofiber membrane with a pore-size hierarchical structure, the problems of poor mechanical strength and low filtration efficiency in the purification of transformer insulation oil are solved, and efficient purification and performance improvement of aging insulation oil is achieved, reducing environmental pollution and maintenance costs.
Patent Information
- Application Number
- CN202411308428.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has poor mechanical strength, low filtration efficiency, large filtration resistance in the purification of transformer insulation oil, and aging insulation oil contains toxic substances, resulting in high environmental pollution and maintenance costs.
A composite nanofiber membrane with a pore-size hierarchical structure was prepared by electrospinning process, combining PVDF, PTFE and BaTiO3 nanoparticles, and using a wire mesh as a substrate to form a gradient porous fiber membrane to enhance mechanical strength and filtration efficiency.
It realizes efficient purification of aging insulating oil, improves acid value, dielectric characteristics and breakdown voltage, reduces the microwater content, improves the service life and mechanical strength of the fiber membrane, and significantly improves the filtration efficiency and accuracy.
Smart Images

Figure CN119041100A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of transformer insulating oil regeneration and purification, and in particular to a composite nanofiber membrane with a graded pore size structure, and a preparation method and application thereof. Background Art
[0002] Insulating oil is an important insulating medium in electrical equipment. It mainly plays the roles of insulation, heat dissipation, cooling and arc extinguishing. Its performance is directly related to whether the power grid can operate safely.
[0003] Insulating oil used for a long time will continue to age under the influence of electromagnetic fields, temperature, oxygen, electric arcs, copper and iron catalysts, and undergo oxidation, cracking and carbonization reactions, generating various impurities, which will reduce its insulation and cooling performance and even cause electrical equipment failures. Therefore, insulating oil needs to be replaced regularly to ensure the safe operation of the power grid. Waste transformer insulating oil contains a large amount of toxic substances. If it is directly discharged, it will cause serious environmental pollution and increase the maintenance cost of the transformer. Therefore, it needs to be safely disposed of or recycled. At present, the commonly used methods for purifying aged insulating oil include vacuum filtration, pressure filtration, adsorption filtration and electrostatic oil purification. The above methods can effectively filter out gas and larger solid impurities in insulating oil and restore its insulation performance to a certain extent. However, the above methods still have problems such as poor mechanical strength, low filtration efficiency and large filtration resistance.
[0004] Nanofiber membranes have the advantages of large fiber specific surface area, small diameter, small pore size and high porosity, and show great potential in the purification of insulating oil. The construction of nanofiber membranes with graded pore size structures can achieve graded filtration of insulating oil and significantly improve filtration efficiency and accuracy. Summary of the invention
[0005] The purpose of the present invention is to provide a composite nanofiber membrane with a pore size classification structure and its preparation method and application, so as to solve the problems existing in the above-mentioned prior art, achieve excellent purification effect of transformer aged insulating oil, and improve the acid value, dielectric, micro-water properties, and breakdown voltage of the purified insulating oil, thereby increasing the service life and mechanical strength of the fiber membrane.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] The present invention provides a method for preparing a composite nanofiber membrane, comprising the following steps:
[0008] (1) preparing an electrospinning precursor solution: mixing PVDF powder and PTFE nanoparticles in a solvent to obtain an electrospinning precursor solution;
[0009] (2) preparing a composite metal mesh: dispersing BaTiO3 nanoparticles in a solvent, depositing the obtained dispersion on a metal mesh by electrostatic spraying, and drying to obtain a composite metal mesh;
[0010] (3) Performing electrospinning with the electrospinning precursor solution, collecting the electrospinning membrane with the composite metal mesh, and obtaining the composite nanofiber membrane.
[0011] Furthermore, the mass percentage of the PVDF powder in the electrospinning precursor solution is 10 wt %, and the mass percentage of the PTFE nanoparticles in the electrospinning precursor solution is 0.1 wt %.
[0012] Furthermore, the mass percentage of the BaTiO3 nanoparticles in the dispersion is 15wt%.
[0013] Furthermore, the particle size of the PTFE nanoparticles is 50-100 nm; the particle size of the BaTiO3 nanoparticles is 40-80 nm.
[0014] Furthermore, the voltage of the electrostatic spraying is 15 to 20 kV; the voltage of the electrostatic spinning is 18 to 20 kV.
[0015] Furthermore, the solvent in step (1) is a mixed solvent of tetrahydrofuran and N,N-dimethylformamide in a mass ratio of 3:2; and the solvent in step (2) is a mixed solution of acetone and N,N-dimethylformamide in a mass ratio of 4:1.
[0016] Furthermore, the metal mesh is made of 304 stainless steel.
[0017] Furthermore, the diameter of the metal wire mesh is 0.05 mm and the aperture is 50 μm.
[0018] The present invention also provides a composite nanofiber membrane prepared by the above preparation method.
[0019] The present invention further provides application of the composite nanofiber membrane in purification of aged mineral insulating oil of transformers.
[0020] The more preferred preparation steps of the present invention are as follows:
[0021] S1. Preparation of spinning precursor solution: In order to prevent PVDF powder from agglomerating during solution preparation and affecting the dissolution of PVDF powder, the PVDF powder is first dried, and then dissolved in a mixed solution of THF and DMF in a mass ratio of 3:2, and then PTFE nanoparticles (particle size of 50-100 nm) are added to make the mass fraction of PTFE nanoparticles 0.1wt.%, the mass fraction of PVDF powder is 10wt.%, and after ultrasonic dispersion, the solution is allowed to stand for degassing to obtain a spinning precursor solution;
[0022] S2. Preparation of composite metal wire mesh: BaTiO3 nanoparticles (particle size of 40-80nm) are dried, and then added into a mixed solution of acetone and DMF in a mass ratio of 4:1, so that the mass fraction of BaTiO3 nanoparticles is 15wt.%, and ultrasonically vibrated for 30-60min to form a dispersion, which is deposited on the metal wire mesh by electrostatic spraying and dried with air.
[0023] The electrostatic spray deposition steps are as follows:
[0024] a. Use a syringe to absorb about 5mL of dispersion liquid, and invert the needle hole to remove all bubbles. After connecting the nozzle, make sure the tail of the piston is in full contact with the peristaltic pump push rod;
[0025] b. Cut a 20cm×20cm metal mesh as the receiving film, and adjust the distance between the nozzle and the receiving surface of the metal mesh;
[0026] c. Connect the nozzle and the metal mesh to positive and negative high-voltage direct current respectively, turn on the temperature control light, set the flow rate to 3-5 mL / h, keep the needle tip 15-20 cm away from the receiving film, and perform electrostatic spray deposition at 25-35°C, 30-40% humidity, and 15-20 kV voltage.
[0027] S3. Preparation of composite nanofiber membrane with graded pore size structure: inject the spinning precursor prepared in step S1 into a syringe for electrospinning, cover the collecting drum with the composite metal wire mesh prepared in step S2 to collect the electrospun membrane, dry at 50-60°C for 3-4h to obtain a composite nanofiber membrane with graded pore size structure.
[0028] The electrospinning steps are as follows:
[0029] (1) Use a syringe to draw about 8 mL of spinning precursor solution, and invert the needle hole to remove all bubbles in it. After connecting the metal needle, make the tail of the piston fully contact with the peristaltic pump push rod;
[0030] (2) Covering the collecting drum with the metal wire mesh prepared in step S2 to collect the electrospun membrane;
[0031] (3) Connect the syringe metal needle and the metal wire mesh to positive and negative high-voltage direct current respectively, turn on the temperature control lamp, set the liquid flow rate to 0.5-0.75 mL / h, set the needle tip to 10-15 cm from the receiving surface, and perform electrospinning at 35±0.5°C and a voltage of 18-20 kV to obtain a composite nanofiber membrane with a graded pore size structure.
[0032] Preferably, the diameter of the metal mesh is 0.05 mm and the aperture is 50 μm.
[0033] The present invention constructs a gradient porous fiber membrane with a gradually shrinking pore size from front to back to balance the filtration efficiency and the pressure drop. PTFE has a low surface energy, and PTFE nanoparticles are evenly dispersed in a PVDF solution, which not only reduces the surface energy of the fiber membrane, but also increases the roughness, and can effectively enhance the hydrophobicity of the fiber membrane. The nanofibers are compounded with a metal mesh, and the interaction between a high-voltage electric field and the metal mesh is utilized to expand the inhomogeneity of the electric field, so that the nanofibers are arranged in an orderly manner, and a graded pore size structure is realized. The metal mesh is electrostatically sprayed to deposit BaTiO3 nanoparticles, so that the metal mesh has a electret effect, and the surface roughness is also increased, so that the nanofibers are more firmly attached.
[0034] The present invention discloses the following technical effects:
[0035] The present invention composites a metal wire mesh as a substrate on the basis of a single nanofiber membrane to enhance the mechanical strength and environmental tolerance of the fiber membrane. The combined use of two electret materials can achieve a rich surface potential of the filter material and enhance the interception effect of electrostatic action on fine particles. The fiber membrane with pore size classification can maintain low pressure drop and stable and long-lasting filtration performance to achieve efficient filtration.
[0036] The composite nanofiber membrane of the present invention has excellent comprehensive performance and is suitable for deep removal of impurities from aged insulating oil. It can remove common impurities and moisture in aged insulating oil, reduce its acid value, and improve the dielectric properties of insulating oil. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 Schematic diagram of the front and back sides of the composite nanofiber membrane with graded pore size structure prepared in Example 1: (a) front side, (b) back side. DETAILED DESCRIPTION
[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0040] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0044] Example 1
[0045] S1. Prepare a spinning precursor solution: dry the PVDF powder at 60°C for 24h, then dissolve the PVDF powder in a mixed solution of THF and DMF in a mass ratio of 3:2, then add PTFE nanoparticles (particle size of 100nm) to make the mass fraction of PTFE nanoparticles 0.1wt.%, the mass fraction of PVDF powder 10wt.%, and ultrasonically disperse at room temperature, then stand for degassing to obtain a spinning precursor solution;
[0046] S2. Preparation of composite metal wire mesh: BaTiO3 nanoparticles (particle size of 50nm) are dried, and then added into a container filled with a mixed solution of acetone and DMF in a mass ratio of 4:1, so that the mass fraction of BaTiO3 nanoparticles is 15wt.%, and the container is sealed with a sealing film, ultrasonically vibrated for 30 minutes to form a dispersion, which is deposited on the metal wire mesh by electrostatic spraying and dried with air.
[0047] The electrostatic spray deposition steps are as follows:
[0048] a. Use a syringe to absorb about 5mL of dispersion liquid, and invert the needle hole to remove all bubbles. After connecting the nozzle, make sure the tail of the piston is in full contact with the peristaltic pump push rod;
[0049] b. Cut a 20cm×20cm piece of 304 stainless steel wire mesh (0.05mm in diameter, 50μm in aperture) as the receiving film, and adjust the distance between the nozzle and the receiving surface of the wire mesh;
[0050] c. Connect the nozzle and the metal mesh to positive and negative high-voltage direct current respectively, turn on the temperature control light, set the flow rate to 4mL / h, keep the needle tip 15cm away from the receiving film, and perform electrostatic spray deposition at 35±0.5℃, 40% humidity, and 20kV voltage.
[0051] S3. Preparation of a composite nanofiber membrane with a graded pore size structure: inject the spinning precursor prepared in step S1 into a syringe for electrospinning, cover the collecting roller with the composite metal wire mesh prepared in step S2 to collect the electrospun membrane, and then dry it at 50°C for 4 hours to obtain a composite nanofiber membrane with a graded pore size structure.
[0052] The electrospinning steps are as follows:
[0053] (1) Use a syringe (the inner diameter of the metal needle of the syringe is 0.8 mm) to draw about 8 mL of spinning precursor solution, and invert the needle hole to remove all bubbles in it. After connecting the metal needle, make the tail of the piston fully contact with the push rod of the peristaltic pump;
[0054] (2) Covering the collecting drum with the metal wire mesh prepared in step S2 to collect the electrospun membrane;
[0055] (3) Connect the metal needle of the syringe and the metal wire mesh to positive and negative high-voltage direct current respectively, turn on the temperature control lamp, set the liquid inlet flow rate to 0.75 mL / h, set the needle tip to 15 cm from the receiving surface, perform electrospinning for 1 h at 35±0.5°C, relative humidity 40±2% RH, and voltage 20 kV, and then dry at 50°C for 4 h to obtain a composite nanofiber membrane with a graded pore size structure.
[0056] Surface morphology of the composite nanofiber membrane with graded pore size prepared in Example 1:
[0057] The fiber membrane was fixed on the sample stage with conductive glue and placed in a vacuum environment for gold plating on the fiber membrane surface. The sample was then transferred to the scanning electron microscope, and the sample morphology was observed at an accelerating voltage of 10 kV. The magnification was adjusted and the pictures were taken and stored. The results are as follows: Figure 1 shown.
[0058] Depend on Figure 1 It can be seen that the fiber membrane made by the electrospinning process with the metal mesh as the receiver has a morphology similar to that of a leaf, showing different structural characteristics on both sides. Among them, the fiber membrane close to the metal mesh side is called the front side, and the fiber membrane away from the metal mesh side is called the back side. It was found through observation that the fibers on the back side of the composite nanofiber membrane were randomly arranged, and the pores between the fibers were small and uniform. In contrast, the fibers on the front side of the membrane were more oriented, and the pores between the fibers were distributed in a polarity of large pores and small pores. The different structural characteristics on both sides of the composite nanofiber membrane are attributed to the interaction between the high-voltage electric field and the metal mesh. The fibers inside the metal mesh and their intersections show a stronger attraction to the spinning solution, so the fibers preferentially attach to the metal fibers and their intersections, thereby forming a patterned nanofiber layer with an excellent arrangement structure. With the further development of the electrospinning process, the directional attraction of the metal mesh to the fibers gradually weakens, so the subsequently attached nanofiber layer gradually presents a randomly arranged structure.
[0059] Comparative Example 1
[0060] The only difference from Example 1 is that the mass fraction of PTFE nanoparticles in step S1 is 0.2 wt.%.
[0061] Comparative Example 2
[0062] The only difference from Example 1 is that the particle size of the PTFE nanoparticles is 1 μm.
[0063] Comparative Example 3
[0064] The only difference from Example 1 is that the mass fraction of the added BaTiO3 particles is 20wt%.
[0065] Comparative Example 4
[0066] The only difference from Example 1 is that the particle size of the BaTiO3 nanoparticles is 200 nm.
[0067] Purification performance test of aged mineral insulating oil:
[0068] The composite nanofiber membranes prepared in Example 1 and Comparative Examples 1 to 4 were cut into circular membranes with a diameter of 50 mm, and aged mineral insulating oil was purified by a suction filtration device (sand core diameter of 41 mm, vacuum degree of -0.1 MPa), with non-woven fabric as a blank control. The acid value, dielectric loss, micro-water content and breakdown voltage of the insulating oil before and after purification were measured respectively.
[0069] The mineral insulating oil used in the experiment is Karamay 25# transformer mineral insulating oil. Its main performance parameters before delivery are shown in Table 1, its main performance parameters after aging are shown in Table 2, and its main performance parameters after purification by the composite nanofiber membrane of the embodiment and the comparative example are shown in Table 3.
[0070] Table 1
[0071]
[0072] Table 2
[0073]
[0074] Table 3
[0075]
[0076]
[0077] It can be seen from the data in Table 3 that when no nanoparticles are added to the blank group and non-woven fabric is used as the receiving substrate, the pure PVDF nanofiber membrane still has a certain degree of purification effect on the aged insulating oil, but the performance of the purified insulating oil is still far behind that of the unused insulating oil, and the filtration rate is slower than that of Example 1. The composite nanofiber membrane with a graded pore size structure prepared in the embodiment of the present invention can effectively improve the properties of the natural ester insulating oil after purification, such as breakdown strength, dielectric loss performance, and micro-water content, and can significantly improve the filtration efficiency to meet the requirements of the standard.
[0078] Compared with Example 1, the mass fraction and particle size of PTFE particles in Comparative Examples 1 and 2 have changed, and the breakdown strength of the corresponding purified insulating oil is lower than that in Example 1, while the dielectric loss, micro-water content and acid value are all higher than those in Example 1. This indicates that when the PTFE particle content is too high and the particle size is too large, the degree of dispersion is reduced, and agglomeration occurs in the fiber membrane, which reduces the hydrophobicity and electret properties of the fiber membrane, thereby reducing the acid product, impurity and moisture removal performance of the composite fiber membrane.
[0079] Compared with Example 1, the mass fraction and particle size of the BaTiO3 particles sprayed on the metal wire mesh in Comparative Examples 3 and 4 have changed, and the performance indicators of the corresponding purified insulating oil have decreased compared with those in the example. This shows that higher mass fraction and particle size may affect the electric field polarization effect brought by the metal wire mesh, resulting in changes in the directional arrangement of the fiber pore size. The larger particle size also slows down the filtration rate, which may be because the nanoparticles have blocked part of the gaps in the metal wire mesh, resulting in a lower porosity.
[0080] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a composite nanofiber membrane, characterized in that: The following steps are involved: (1) preparing an electrospinning precursor solution: mixing PVDF powder and PTFE nanoparticles in a solvent to obtain an electrospinning precursor solution; (2) preparing a composite metal mesh: dispersing BaTiO3 nanoparticles in a solvent, depositing the obtained dispersion on a metal mesh by electrostatic spraying, and drying to obtain a composite metal mesh; (3) Performing electrospinning with the electrospinning precursor solution, collecting the electrospinning membrane with the composite metal mesh, and obtaining the composite nanofiber membrane.
2. The preparation method according to claim 1, characterized in that: The mass percentage of the PVDF powder in the electrospinning precursor solution is 10 wt %, and the mass percentage of the PTFE nanoparticles in the electrospinning precursor solution is 0.1 wt %.
3. The preparation method according to claim 1, characterized in that: The mass percentage of the BaTiO3 nanoparticles in the dispersion is 15wt%.
4. The preparation method according to claim 1, characterized in that: The particle size of the PTFE nanoparticles is 50-100 nm; the particle size of the BaTiO3 nanoparticles is 40-80 nm.
5. The preparation method according to claim 1, characterized in that: The voltage of the electrostatic spraying is 15-20 kV; the voltage of the electrostatic spinning is 18-20 kV.
6. The preparation method according to claim 1, characterized in that: The solvent in step (1) is a mixed solvent of tetrahydrofuran and N,N-dimethylformamide in a mass ratio of 3:2; and the solvent in step (2) is a mixed solvent of acetone and N,N-dimethylformamide in a mass ratio of 4:
1.
7. The preparation method according to claim 1, characterized in that: The metal wire mesh is made of 304 stainless steel.
8. The preparation method according to claim 7, characterized in that: The diameter of the metal wire mesh is 0.05 mm and the aperture is 50 μm.
9. The composite nanofiber membrane prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the composite nanofiber membrane as claimed in claim 9 in purifying aged mineral insulating oil of transformers.
Citation Information
Patent Citations
Method for preparing high dielectric constant polymer-based nano composite material
CN103147226A
Solid-state polymer electrolyte membrane with grid structure, and preparation method thereof
CN112259788A
Preparation method and application of long-acting charged and aperture-graded nano film
CN115287823A
Composite nanofiber membrane as well as preparation method and application thereof
CN115976740A
Composite nanofiber membrane as well as preparation method and application thereof
CN117679975A
Cited By
Nano-modified composite fiber filter membrane based on HAP as well as preparation method and application of nano-modified composite fiber filter membrane
CN119656882A
Surface-modified composite fiber filter membrane as well as preparation method and application thereof
CN119656891A