Lamellar metal organic framework modified carbon fiber as well as preparation method and application thereof
By preparing sheet-like metal-organic frameworks on the surface of carbon fibers, the problem of poor interfacial bonding between carbon fibers and epoxy resins was solved, resulting in carbon fiber/epoxy resin composites with high water resistance and mechanical properties, thus improving erosion resistance in marine environments.
Patent Information
- Application Number
- CN202411529972.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
AI Technical Summary
The smooth surface of carbon fiber has poor wettability and poor interfacial bonding performance with epoxy resin matrix, which leads to accelerated deterioration of carbon fiber reinforced composite coatings in marine environment and reduces the safe service life of marine engineering equipment.
A sheet-like metal-organic framework modified carbon fiber was prepared on the surface of carbon fiber by in-situ growth method. By reacting carbon oxide with cobalt source and dimethylimidazole in water, a sheet-like ZIF-67 structure was formed, which enhanced the interfacial bonding between carbon fiber and epoxy resin.
It improves the water resistance and mechanical properties of carbon fiber/epoxy resin composites, enhances the interfacial bonding strength, improves the erosion resistance of composites, and extends the service life in marine environments.
Smart Images

Figure CN119041207A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a sheet metal organic framework modified carbon fiber and a preparation method and application thereof. Background Art
[0002] Carbon fiber materials are widely used in aerospace, engineering construction, and marine equipment due to their light weight, high specific strength and modulus, and good wear resistance. However, the surface of carbon fiber is smooth and has poor wettability. It is chemically inert and has poor interfacial bonding performance with the epoxy resin matrix, which limits the application of carbon fiber reinforced composite coatings in the field of metal protection. In the marine environment of high temperature, high humidity, and high salt fog, the carbon fiber reinforced composite coating is affected by continuous wave slapping, tidal surges, and silt erosion. The strong coupling damage of environmental factors and corrosive media acts on the surface of the carbon fiber reinforced composite coating, the carbon fiber / resin interface, and the metal matrix / resin interface, causing the composite coating to deteriorate and fail rapidly, greatly reducing the safe service life of marine equipment.
[0003] In order to enhance the interfacial bonding strength between carbon fiber and resin matrix, carbon fiber needs to be surface treated to increase the chemical activity and roughness of carbon fiber surface, reduce defects at the interface, and achieve high-strength bonding between fiber / resin interface. Currently, commonly used carbon fiber surface modification methods include oxidation, sizing agent modification, grafting and nanoparticle modification. Among them, oxidation method helps to increase the chemical activity of fiber surface, but excessive oxidation etching can easily damage the intrinsic structure of carbon fiber. Traditional sizing agents have low heat resistance and solvents are easy to volatilize, so the interfacial bonding performance between carbon fiber / resin is weak. However, nanoparticle modification method helps to fill the surface defects of carbon fiber and bridge the carbon fiber and resin matrix, which helps to form a good stress transfer network.
[0004] Metal-organic frameworks (ZIFs) have the characteristics of high porosity, specific surface area and adjustable pore size and have been widely used in anti-corrosion coatings, adsorbents, gas separation agents and catalysts. 2+ ) and dimethylimidazole to form a zeolite imidazolate framework (ZIF-67), which is easy to synthesize at room temperature without the use of high temperatures and toxic organic solvents. At the same time, ZIF-67 nanoparticles can be loaded with corrosion inhibitors and functionalized to enhance the corrosion resistance of epoxy coatings. However, its water resistance is very poor and it is easily hydrolyzed, resulting in huge challenges in practical applications, especially in seawater environments. Summary of the invention
[0005] The main purpose of the present invention is to provide a lamellar metal organic framework modified carbon fiber and its preparation method and application, so as to overcome the shortcomings of ZIF-67 dissolving in aqueous solution, easy structural collapse and difficulty in chemical modification.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: The embodiment of the present invention provides a method for preparing a sheet metal organic framework modified carbon fiber, which comprises: Degreasing, desizing and oxidizing the carbon fiber to obtain oxidized carbon fiber; And, a first mixed reaction system including oxidized carbon fiber, a cobalt source, dimethylimidazole and water is reacted to obtain a sheet metal organic framework modified carbon fiber.
[0007] The embodiment of the present invention also provides a lamellar metal organic framework modified carbon fiber obtained by the aforementioned preparation method, wherein the lamellar metal organic framework modified carbon fiber comprises carbon fiber and flaky ZIF-67 grown on the surface of the carbon fiber.
[0008] An embodiment of the present invention also provides a water-resistant carbon fiber / epoxy resin composite coating, which is obtained by mixing the aforementioned lamellar metal organic framework modified carbon fiber, epoxy resin and curing agent and applying them to the surface of the substrate for curing treatment.
[0009] The embodiment of the present invention also provides a water-resistant carbon fiber / epoxy resin composite material, which is obtained by mixing the aforementioned lamellar metal organic framework modified carbon fiber, epoxy resin and curing agent and performing a curing treatment.
[0010] The embodiments of the present invention also provide the use of the aforementioned lamellar metal organic framework modified carbon fiber, water-resistant carbon fiber / epoxy resin composite coating or water-resistant carbon fiber / epoxy resin composite material in the preparation of marine engineering equipment.
[0011] Compared with the prior art, the present invention has the following beneficial effects: (1) The water-resistant carbon fiber / epoxy resin composite material of the present invention has strong water resistance, high mechanical properties and erosion resistance, and can be used for a long time in a marine environment; (2) In the present invention, the sheet metal organic framework modified carbon fiber, epoxy resin and curing agent are mixed and coated on the surface of the metal substrate to isolate the substrate from the external environment, thereby improving the erosion resistance of the carbon fiber reinforced composite material; (3) The preparation method of the water-resistant carbon fiber / epoxy resin composite material provided by the present invention is relatively simple and mature, and the high-strength interface bonding between the fiber and the epoxy resin makes the composite material have excellent mechanical properties and excellent erosion resistance; (4) The highly water-resistant lamellar metal organic framework modified carbon fiber of the present invention not only helps to form a mechanical meshing effect between the carbon fiber and the epoxy resin, but also helps to reduce the modulus mismatch problem between the carbon fiber and the epoxy resin, thereby improving the interface bonding performance between the carbon fiber and the resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0013] Figure 1 is a scanning electron microscope image of the oxidized carbon fiber in Example 1 of the present invention; Figure 2 This is a scanning electron microscope image of the sheet-like metal organic framework structure L1-ZIF-67 modified carbon fiber in Example 1 of the present invention; Figure 3 This is a scanning electron microscope image of the sheet-like metal organic framework structure L2-ZIF-67 modified carbon fiber in Comparative Example 3 of the present invention; Figure 4 This is a scanning electron microscope image of the dodecahedral metal organic framework D-ZIF-67 modified carbon fiber in Comparative Example 4 of the present invention; Figure 5 The XRD spectra of carbon fibers under different modification processes in Example 1, Comparative Example 2 and Comparative Example 4 of the present invention are shown; Figure 6 1 is a tensile stress-strain curve of a carbon fiber reinforced epoxy composite material under different modification processes in one embodiment of the present invention; Figure 7 The morphology diagram of the tensile fracture interface of the carbon fiber reinforced epoxy composite material under different modification processes in one embodiment of the present invention; Figure 8 These are morphology diagrams of different carbon fibers after being immersed in aqueous solution for 0 h and 24 h in one embodiment of the present invention.
[0014] Fig. 9 Graph showing mass loss of different carbon fibers after erosion in one embodiment of the present invention. DETAILED DESCRIPTION
[0015] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The present invention provides a method for enhancing the interfacial performance of carbon fiber / epoxy resin by using a highly water-resistant sheet metal organic framework structure. A highly water-resistant sheet L-ZIF-67 is prepared on the surface of carbon fiber by an in-situ growth method, which provides a new idea for the preparation of erosion-resistant coatings for steel pipe piles in marine environments.
[0016] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] Specifically, as one aspect of the technical solution of the present invention, a method for preparing a sheet metal organic framework modified carbon fiber involves: Degreasing, desizing and oxidizing the carbon fiber to obtain oxidized carbon fiber; And, a first mixed reaction system including oxidized carbon fiber, a cobalt source, dimethylimidazole and water is reacted to obtain a sheet metal organic framework modified carbon fiber.
[0018] In some preferred embodiments, the preparation method specifically includes: mixing the oxidized carbon fiber with a cobalt source aqueous solution and ultrasonicating for 30-60 minutes, then adding a dimethylimidazole aqueous solution and letting it react for 6-12 hours, and then washing and drying to obtain uniformly grown lamellar metal-organic framework modified carbon fibers.
[0019] Furthermore, the mass ratio of the oxidized carbon fiber to the cobalt source is (0.5-1):(0.1-0.2).
[0020] Furthermore, the molar ratio of the cobalt source to dimethylimidazole is (0.4-0.7):(4-5).
[0021] In some preferred embodiments, the preparation method specifically comprises: mixing the oxidized carbon fiber with an excess cobalt source aqueous solution and performing ultrasound for 30-60 minutes, then adding a dimethylimidazole aqueous solution and standing for reaction for 6-12 hours, and then washing and drying to obtain an overgrown sheet metal organic framework modified carbon fiber; Wherein, the mass ratio of the oxidized carbon fiber to the cobalt source is (0.5-1):(0.3-0.4); the molar ratio of the cobalt source to dimethylimidazole is (1.2-1.5):(4-5).
[0022] In some preferred embodiments, the cobalt source includes cobalt nitrate hexahydrate and / or cobalt chloride hexahydrate, but is not limited thereto.
[0023] In some preferred embodiments, the preparation method of dodecahedral metal organic framework modified carbon fiber includes: mixing the oxidized carbon fiber with a cobalt source methanol solution and ultrasonicating for 30-60 minutes, then adding a methanol solution of dimethylimidazole and polyvinyl pyrrolidone and letting it react for 6-12 hours, and then washing and drying to obtain the dodecahedral metal organic framework modified carbon fiber.
[0024] Furthermore, the mass ratio of the oxidized carbon fiber to the cobalt source is (0.5-1):(0.1-0.2).
[0025] Furthermore, the molar mass ratio of the cobalt source, dimethylimidazole and polyvinyl pyrrolidone is (0.4-0.7) mmol: (4-5) mmol: (0.1-0.4) g.
[0026] In some more specific embodiments, the method for preparing the sheet metal organic framework modified carbon fiber comprises the following steps: S1, immersing the carbon fiber in a sodium hydroxide solution at 70-90°C, stirring at a speed of 200-300 rpm for 2-6 hours, then washing three times with deionized water and drying at 60-80°C to obtain a carbon fiber with deoiled surface; S2, removing the sizing agent on the surface of the carbon fiber by refluxing the acetone organic solvent, stirring at a speed of 300-350 rpm for 4-8 hours, washing three times with deionized water and drying at 60-80° C. to obtain the desizing carbon fiber; S3, immersing the desizing carbon fiber powder in 100-300 ml of concentrated nitric acid, stirring at a constant speed for 4-6 hours at a temperature of 75-85° C., washing and refluxing to obtain nitric acid-oxidized carbon fiber; S4, adding the oxidized carbon fiber powder obtained in S3 to a cobalt nitrate hexahydrate aqueous solution and ultrasonicating for 30 minutes, wherein the mass ratio of the oxidized carbon fiber to the cobalt nitrate hexahydrate is (0.5-1) g:(0.1-0.2) g; S5. Slowly drop a dimethylimidazole aqueous solution into the above S4 solution, let it stand for 12 hours after the dropwise addition is completed, pour off the upper solvent, wash with deionized water and pour off the upper solvent again, repeat the above steps 3-4 times; then dry in an oven at 60-80° C. to obtain an in-situ grown sheet metal organic framework modified carbon fiber with strong water resistance; wherein the molar ratio of cobalt nitrate hexahydrate to dimethylimidazole is (0.4-0.7) mmol:(4-5) mmol; S6. Add the oxidized carbon fiber powder obtained in S3 into a cobalt nitrate hexahydrate methanol solution and ultrasonicate for 30 minutes, wherein the mass ratio of the oxidized carbon fiber to the cobalt nitrate hexahydrate is (0.5-1) g:(0.1-2) g.
[0027] Another aspect of the embodiments of the present invention further provides a lamellar metal organic framework modified carbon fiber obtained by the aforementioned preparation method, wherein the lamellar metal organic framework modified carbon fiber comprises carbon fiber and flaky ZIF-67 grown on the surface of the carbon fiber.
[0028] Furthermore, the lamellar metal organic framework modified carbon fiber includes a lamellar metal organic framework modified carbon fiber with flaky ZIF-67 uniformly grown on the surface.
[0029] Furthermore, the surface-grown flaky ZIF-67 includes two states: uniform growth (L1-ZIF-67) and excess growth (L2-ZIF-67).
[0030] Furthermore, the surface-grown flake ZIF-67 is uniformly grown (L1-ZIF-67).
[0031] Another aspect of an embodiment of the present invention further provides a water-resistant carbon fiber / epoxy resin composite coating, which is obtained by mixing the aforementioned lamellar metal organic framework modified carbon fiber, epoxy resin and curing agent and applying (coating) them to the surface of the substrate for curing treatment.
[0032] Further, the epoxy resin includes phenolic E51 epoxy resin and / or glycidylamine epoxy resin 1070, but is not limited thereto.
[0033] Further, the curing agent includes alicyclic amine epoxy resin curing agent 1618 and / or phthalic anhydride, but is not limited thereto.
[0034] Furthermore, the curing treatment is carried out at a temperature of 60-80°C and for a time of 10-12 hours.
[0035] Furthermore, the composite coating has a thickness of 100-200 μm.
[0036] Another aspect of an embodiment of the present invention further provides a water-resistant carbon fiber / epoxy resin composite material, which is obtained by mixing the aforementioned lamellar metal organic framework modified carbon fiber, epoxy resin and curing agent and performing a curing treatment.
[0037] Further, the epoxy resin includes phenolic E51 epoxy resin and / or glycidylamine epoxy resin 1070, but is not limited thereto.
[0038] Further, the curing agent includes alicyclic amine epoxy resin curing agent 1618 and / or phthalic anhydride, but is not limited thereto.
[0039] Furthermore, the curing treatment is carried out at a temperature of 60-80°C and for a time of 10-12 hours.
[0040] Furthermore, the size of the composite material is 80×20×4 mm.
[0041] Another aspect of the embodiments of the present invention further provides the use of the aforementioned lamellar metal organic framework modified carbon fiber, water-resistant carbon fiber / epoxy resin composite coating or water-resistant carbon fiber / epoxy resin composite material in the preparation of marine engineering equipment.
[0042] The present invention provides a design method for reinforcing the interface bonding strength of carbon fiber / epoxy resin composite materials with a highly water-resistant sheet metal organic framework structure material, which can be used in a marine environment for a long time and has high mechanical properties, erosion resistance and corrosion resistance, and correspondingly provides a preparation method of the coating. It includes: A high-performance fiber-reinforced coating is obtained through the fiber and epoxy resin composite technology, and a carbon fiber powder with strong water resistance is obtained by modifying the surface of the carbon fiber using a metal-organic framework structure material. In addition, a strong and integrated high-performance fiber-reinforced composite coating is obtained by compounding the modified carbon fiber powder with epoxy resin.
[0043] The lamellar metal organic framework modified carbon fiber in the present invention can not only increase the surface roughness of the carbon fiber and improve the wettability with epoxy resin, but also make the organic structure less likely to collapse; at the same time, the composite material and composite coating prepared from the modified carbon fiber have excellent mechanical strength and impact resistance, thereby improving its service life in the field of metal protection in marine environment.
[0044] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0045] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0046] Example 1: Preparation of L1-ZIF@CF / EP in the present invention S1. Weigh 10g of carbon fiber powder and immerse it in 500ml of sodium hydroxide solution (2M), and stir it at 80℃ for 2h. After the reaction, wash it with water three times and dry it; S2, immerse 10g of the deoiled carbon fiber powder in 500ml of acetone organic solvent, reflux and stir at 60°C for 4h; after the reaction is completed, wash with water three times and dry; S3, immerse 10g of the desizing carbon fiber powder in 250ml of concentrated nitric acid, reflux and stir at 80°C for 6h; after the reaction is completed, dilute it 20 times and remove the supernatant, wash the precipitated carbon fiber powder with water three times and dry it; S4, weigh 0.19g of cobalt nitrate hexahydrate and dissolve it in 50ml of aqueous solution, add 0.8g of carbon fiber powder and ultrasonicate for 30min to obtain a precursor solution, weigh 0.35g of dimethylimidazole and dissolve it in 50ml of aqueous solution, and ultrasonicate for 30min to obtain solution B; S5. Slowly add liquid B to the above precursor solution, let it stand for 12 hours after the addition is completed, remove the upper solvent, repeatedly wash with deionized water and retain the precipitate; then dry at 60°C to obtain an in-situ grown lamellar metal organic framework modified carbon fiber (L1-ZIF-67@CF); 0.5 g of L1-ZIF-67@CF was added to a mixture of 12.1 g of E51 epoxy resin and 7.2 g of epoxy resin curing agent 1618, and the air in the mixture was evacuated in a vacuum mixer; the mixture was poured into a mold of 80×20×4 mm and cured at 80°C to form a L1-ZIF-67@CF reinforced composite material.
[0047] Comparative Example 1: Preparation of the pure epoxy composite material of the present invention S1. Take 12.1 g of E51 epoxy resin and 7.2 g of epoxy resin curing agent 1618, mix and stir, and extract the air in the mixture in a vacuum mixer; pour the mixture into a mold of 80×20×4 mm and cure it at 80° C. to form a pure epoxy composite material.
[0048] Comparative Example 2: Preparation of the carbon fiber reinforced epoxy composite material of the present invention S1. Referring to the methods of S1-S3 in Example 1, obtaining carbon fiber powder after nitric acid oxidation; S2. Take 0.5 g of CFO powder and add it to a mixture of 12.1 g of E51 epoxy resin and 7.2 g of epoxy resin curing agent 1618, and evacuate the air in the mixture in a vacuum mixer; pour the mixture into a mold of 80×20×4 mm and cure it at 80° C. to form a CFO reinforced resin composite material.
[0049] Compared with Example 1, only the carbon fiber was subjected to surface oxidation treatment, and the tensile mechanical properties of the oxidized carbon fiber reinforced resin composite material were tested. The test results are as follows: Figure 6 As shown in Figure 2, the tensile fracture interface morphology of oxidized carbon fiber / resin is as follows: Figure 7 As shown in the figure, the surface of carbon fiber oxidized by nitric acid is smooth with few grooves. When the composite material is tensilely damaged, the oxidized carbon fiber is pulled out of the resin matrix and separated from the interface between the resin matrix, indicating that it is difficult to effectively enhance the interfacial bonding strength between the fiber and the resin by only surface oxidation treatment of the carbon fiber.
[0050] Comparative Example 3: Preparation of the L2-ZIF-67@CF / EP composite material of the present invention S1. Referring to the methods of S1-S3 in Example 1, obtaining carbon fiber powder after nitric acid oxidation; S2, the following steps are different in that the 0.19 g of cobalt nitrate hexahydrate and 0.35 g of dimethylimidazole weighed in S4 in Example 1 are replaced with 0.5 g of cobalt nitrate hexahydrate and 1.05 g of dimethylimidazole, and L2-ZIF-67@CF is obtained after the reaction is completed; S3. Take 0.5 g of L2-ZIF-67@CF and add it to a mixture of 12.1 g of E51 epoxy resin and 7.2 g of epoxy resin curing agent 1618, and extract the air in the mixture in a vacuum mixer; pour the mixture into a mold of 80×20×4 mm and cure it at 80°C to form a L2-ZIF-67@CF reinforced composite material.
[0051] Comparative Example 4: Preparation of D-ZIF-67@CF / EP composite material S1. Referring to the methods of S1-S3 in Example 1, obtaining carbon fiber powder after nitric acid oxidation; S2, the following steps are different in that the aqueous dimethylimidazole solution in S4 in Example 1 is replaced with a methanol solution of dimethylimidazole and polyvinyl pyrrolidone, and after the reaction is completed, an in-situ grown dodecahedral metal organic framework modified carbon fiber (D-ZIF-67@CF) is obtained; S3. Take 0.5 g of D-ZIF-67@CF and add it to a mixture of 12.1 g of E51 epoxy resin and 7.2 g of epoxy resin curing agent 1618, and evacuate the air in the mixture in a vacuum mixer; pour the mixture into a mold of 80×20×4 mm and cure it at 80°C to form a D-ZIF-67@CF@CF reinforced composite material.
[0052] Performance tests were performed on Example 1 and Comparative Examples 1-4: 1. Structural Characterization Figure 1-Figure 4 The scanning electron microscope images of the oxidized carbon fiber CFO, the sheet metal organic framework material modified carbon fiber (L1-ZIF-67@CF and L2-ZIF-67@CF) and the dodecahedral metal organic framework structure modified carbon fiber D-ZIF-67@CF; for comparative example 2, CFO has a very smooth surface; for example 1, when ZIF-67 and Co are prepared in aqueous solution 2+ When the molar mass is about 0.6 mmol, the carbon fiber surface grows into a uniform sheet-like ZIF-67 structure (L1-ZIF-67@CF); for Comparative Example 3, when ZIF-67 is prepared in aqueous solution and Co 2+ When the molar mass is about 3 mmol, the carbon fiber surface grows into an excessive and uneven sheet-like ZIF-67 structure (L2-ZIF-67@CF); for Comparative Example 4, when ZIF-67 is prepared in methanol solution and Co 2+When the molar mass is about 0.6 mmol, a uniform dodecahedral ZIF-67 structure (D-ZIF-67@CF) grows on the carbon fiber surface.
[0053] Figure 5 The XRD patterns of oxidized carbon fiber CFO, sheet metal organic framework structure modified carbon fiber (L1-ZIF-67@CF) and dodecahedral metal organic framework structure material modified carbon fiber D-ZIF-67@CF; Figure 5 It can be seen that CFO, L1-ZIF-67@CF and D-ZIF-67@CF samples all show two broad diffraction peaks at around 25° and 43°, which correspond to the (002) and (100) crystal planes of carbon. Compared with CFO, L1-ZIF-67@CF and D-ZIF-67@CF samples show obvious diffraction peaks at 2θ of around 7°, 10°, 12°, 14° and 16°, corresponding to the (011), (002), (112), (022), (013) and (222) crystal planes of ZIF-67 crystal, respectively. The XRD spectrum shows that the ZIF-67 structure grows uniformly on the carbon fiber surface, and L1-ZIF-67 and D-ZIF-67 have the same crystal structure.
[0054] 2. Mechanical properties test Figure 6 It is shown that the composite material after the uniform sheet metal organic framework structure is grown on the carbon fiber surface has the highest tensile strength. The carbon fiber surface is uniformly covered with the L1-ZIF-67 structure, which can maximize the surface roughness and interface meshing effect. For comparative example 2, the interface bonding performance between the oxidized carbon fiber reinforced composite material and the epoxy resin matrix is poor, and a large amount of oxidized carbon fiber and the resin have interface separation; for comparative example 4, an appropriate amount of dodecahedral metal organic framework structure grows on the carbon fiber surface. Although the surface roughness is improved, the interface is not only damaged by the interface between the carbon fiber and the resin matrix, but also includes the separation of the new interface layer of D-ZIF-67 and the carbon fiber. Therefore, the tensile strength of the D-ZIF-67@CF / EP composite material is not significantly improved. It shows that in the present invention, the uniform sheet metal organic framework modified carbon fiber can effectively enhance the interface bonding strength between the fiber and the resin. Figure 7 These are the morphologies of the tensile fracture interface of carbon fiber reinforced epoxy composites under different modification processes.
[0055] 3. Water resistance test Figure 8The morphology of oxidized carbon fiber CFO, sheet metal organic framework material modified carbon fiber (L1-ZIF-67@CF and L2-ZIF-67@CF) and dodecahedral metal organic framework structure modified carbon fiber D-ZIF-67@CF after immersion in aqueous solution for 0h and 24h is shown. It can be seen that the dodecahedral metal organic framework D-ZIF-67 has poor water resistance, and the surface D-ZIF-67 structure has been completely hydrolyzed after immersion for 24h; while L1-ZIF-67 still has a complete sheet structure after immersion for 24h. Therefore, sheet metal organic framework modified carbon fiber reinforced composite coating is expected to play a practical application in marine environment.
[0056] 4. Erosion resistance test The erosion and wear test was conducted using an erosion test bench, which mainly consists of an air compressor, a sandblasting gun, a mixer chamber and a specimen rack. The test was conducted using a liquid-solid two-phase flow under simulated ocean conditions. The erosion medium consisted of water and SiC particles with a SiC content of 15 wt %. The impact angle was 90° and the test time for each sample was 30 minutes. Before and after the test, each sample was cleaned and weighed. Fig. 9 As shown, introducing carbon fiber into epoxy resin coating can effectively reduce the mass loss of composite coating and better preserve the surface integrity of the erosion area of composite coating. Among them, the carbon fiber composite coating with uniformly grown flake organic framework has the lowest mass loss after erosion (487.30 mg), which is 37% lower than that of pure resin coating (774.30 mg), and has the best anti-erosion performance.
[0057] Example 2: Preparation of L1-ZIF@CF / EP in the present invention S1. Weigh 10g of carbon fiber powder and immerse it in 500ml of sodium hydroxide solution (2M), and stir it at 70℃ for 6h. After the reaction, wash it with water three times and dry it; S2, immerse 10g of the deoiled carbon fiber powder in 500ml of acetone organic solvent, reflux and stir at 70°C for 6h; after the reaction is completed, wash it with water three times and dry it; S3, immerse 10g of the deslurried carbon fiber powder in 250ml of concentrated nitric acid, reflux and stir at 75°C for 6h; after the reaction is completed, dilute it 20 times and remove the supernatant, wash the precipitated carbon fiber powder three times with water and dry it; S4, weigh 0.08g of cobalt nitrate hexahydrate and dissolve it in 50ml of aqueous solution, add 0.8g of carbon fiber powder and ultrasonicate for 30min to obtain a precursor solution, weigh 0.11g of dimethylimidazole and dissolve it in 50ml of aqueous solution, and ultrasonicate for 30min to obtain solution B; S5. Slowly add liquid B to the above precursor solution, let it stand for 12 hours after the addition is completed, remove the upper solvent, repeatedly wash with deionized water and retain the precipitate; then dry at 80°C to obtain an in-situ grown lamellar metal organic framework modified carbon fiber (L1-ZIF-67@CF); S6. Take 0.5 g of L1-ZIF-67@CF and add it to a mixture of 12.1 g of glycidylamine epoxy resin 1070 and 7.2 g of curing agent phthalic anhydride, and evacuate the air in the mixture in a vacuum mixer; pour the mixture into a mold of 80×20×4 mm and cure it at 60°C to form a L1-ZIF-67@CF reinforced composite material.
[0058] Example 3 S1. Weigh 10g of carbon fiber powder and immerse it in 500ml of sodium hydroxide solution (2M), and stir it at 90℃ for 3h. After the reaction, wash it with water three times and dry it; S2, immerse 10g of the deoiled carbon fiber powder in 500ml of acetone organic solvent, reflux and stir at 80°C for 4h; after the reaction is completed, wash with water three times and dry; S3, immerse 10g of the desizing carbon fiber powder in 250ml of concentrated nitric acid, reflux and stir at 85°C for 4h; after the reaction is completed, dilute it 20 times and remove the supernatant, wash the precipitated carbon fiber powder three times with water and dry it; S4, weigh 0.32g of cobalt nitrate hexahydrate and dissolve it in 50ml of aqueous solution, add 0.8g of carbon fiber powder and ultrasonicate for 30min to obtain a precursor solution, weigh 0.94g of dimethylimidazole and dissolve it in 50ml of aqueous solution, and ultrasonicate for 30min to obtain solution B; S5. Slowly add solution B to the above precursor solution, let it stand for 12 hours after the addition is completed, remove the upper solvent, repeatedly wash with deionized water and retain the precipitate; then dry at 70°C to obtain an in-situ grown lamellar metal organic framework modified carbon fiber (L1-ZIF-67@CF); S6. Take 0.5 g of L1-ZIF-67@CF and add it to a mixture of 12.1 g of E51 epoxy resin and 7.2 g of epoxy resin curing agent 1618, and extract the air in the mixture in a vacuum mixer; pour the mixture into a mold of 80×20×4 mm and cure it at 80°C to form a L1-ZIF-67@CF reinforced composite material.
[0059] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0060] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a sheet metal organic framework modified carbon fiber, characterized in that: include: Degreasing, desizing and oxidizing the carbon fiber to obtain oxidized carbon fiber; And, a first mixed reaction system including oxidized carbon fiber, a cobalt source, dimethylimidazole and water is reacted to obtain a sheet metal organic framework modified carbon fiber.
2. The preparation method according to claim 1, characterized in that: Specifically include: The oxidized carbon fiber is mixed with a cobalt source aqueous solution and subjected to ultrasound for 30-60 minutes, then a dimethylimidazole aqueous solution is added and allowed to react for 6-12 hours, and then washed and dried to obtain uniformly grown lamellar metal organic framework modified carbon fibers.
3. The preparation method according to claim 2, characterized in that: The mass ratio of the oxidized carbon fiber to the cobalt source is (0.5-1):(0.1-0.2).
4. The preparation method according to claim 2, characterized in that: The molar ratio of the cobalt source to dimethylimidazole is (0.4-0.7):(4-5).
5. The lamellar metal organic framework modified carbon fiber prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The sheet metal organic framework modified carbon fiber comprises carbon fiber and sheet-like ZIF-67 grown on the surface of the carbon fiber.
6. The sheet metal organic framework modified carbon fiber according to claim 5, characterized in that: The lamellar metal organic framework modified carbon fiber comprises a lamellar metal organic framework modified carbon fiber with flaky ZIF-67 uniformly grown on the surface.
7. A water-resistant carbon fiber / epoxy resin composite coating, characterized in that: The water-resistant carbon fiber / epoxy resin composite coating is obtained by mixing the lamellar metal organic framework modified carbon fiber according to claim 5 or 6, epoxy resin and a curing agent and applying the mixture to the surface of a substrate for curing treatment.
8. The water-resistant carbon fiber / epoxy resin composite coating according to claim 7, characterized in that: The curing treatment is performed at a temperature of 60-80° C. and for a time of 10-12 hours.
9. A water-resistant carbon fiber / epoxy resin composite material, characterized in that: The water-resistant carbon fiber / epoxy resin composite material is obtained by mixing the lamellar metal organic framework modified carbon fiber according to claim 5 or 6, epoxy resin and a curing agent and performing a curing treatment.
10. Use of the lamellar metal organic framework modified carbon fiber according to any one of claims 5-6, the water-resistant carbon fiber / epoxy resin composite coating according to claims 7-8, or the water-resistant carbon fiber / epoxy resin composite material according to claim 9 in the preparation of marine engineering equipment.
Citation Information
Cited By
Explosion-proof resin composite material and preparation method thereof
CN120082170A
Preparation method and application of asphalt-based reinforced carbon fiber composite material based on metal organic framework interface
CN121407261A
Fiber-modified high-toughness corrosion-resistant composite coating with impact damage visualization and preparation method of fiber-modified high-toughness corrosion-resistant composite coating
CN122445250A