Water-lubricated radial bearing based on bush surface layer non-uniform thickness design
By using non-equal thickness design and locking mechanism in water-lubricated tail bearings, combined with material layers such as wear resistance and heat dissipation, stress concentration, wear and heat dissipation problems are solved, the service life is extended and maintenance costs are reduced, and the maintenance costs are reduced. Deliver the demand for low noise operating environment.
Patent Information
- Application Number
- CN202411160851.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing water-lubricated tail bearings have concentrated stress, severe wear, limited heat dissipation capacity, easy corrosion and insufficient sound insulation performance under the conditions of biased load and axis inclination, resulting in short service life and high maintenance costs, which cannot meet the needs of low-noise operating environments.
Water-lubricated radial bearings based on non-equal thickness of the tile surface layer are adopted. By adjusting the thickness of the tile surface layer to increase the contact area, reduce stress concentration, and combine the locking mechanism to achieve rapid replacement and flexible combination, using wear-resistant and elastic buffering, Heat dissipation, anti-static and corrosion-resistant material layers to optimize bearing performance.
Effectively reduce stress concentration and wear, extend service life, reduce maintenance costs, improve the performance of bearings in high humidity and extreme environments, and meet the needs of low noise operation.
Smart Images

Figure CN119042230A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sliding bearings, in particular to a water-lubricated radial bearing based on a non-uniform thickness design of a tile surface layer. Background Art
[0002] The water-lubricated stern bearing is an important part of the ship's propulsion shaft system, supporting the weight of the stern shaft and propeller. With the increase in ship tonnage, the propeller shaft bends and the axis tilts under the weight of the propeller, causing a large edge load on the stern bearing, that is, a large local load, which seriously affects the performance of the stern bearing. How to improve the bearing lubrication, friction and vibration characteristics under eccentric load and axis tilt is an important problem currently faced by large ships.
[0003] Generally, water-lubricated tail bearings are composed of non-metallic tile surface layer (or "lining") and metal matrix (or "bushing"). At present, water-lubricated tail bearings have a variety of structural forms and material types. According to the relationship between the tile surface layer and the matrix, they can be divided into integral type and slat type; according to the position and number of water grooves, they can be divided into full groove and partial groove. The former has water grooves distributed at equal intervals around the circumference, while the latter has water grooves only set on the upper part of the bearing, and there is no water groove on the lower part of the bearing; the tile surface material mainly includes synthetic nitrile rubber, modified rubber and composite polymer materials.
[0004] However, existing bearings face a number of challenges, especially when dealing with off-center loading and uneven axial loads. Off-center loading refers to uneven load distribution caused by axis tilt or installation errors. Under these conditions, the bearing pad surface layer often experiences uneven pressure distribution, which can increase wear on the pad surface layer, reduce the service life of the bearing, and increase maintenance costs. At the same time, since the ship's stern bearing generates a lot of heat energy during operation, the existing bearings have limited heat dissipation capacity and cannot effectively conduct and dissipate heat, which causes the bearing to overheat, affecting performance and safety. Especially in salt water environments, the limited bearings are easily corroded and have insufficient sound insulation performance, which cannot meet the current demand for a low-noise operating environment, thereby increasing the cost of bearing use. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a water-lubricated radial bearing based on a non-uniform thickness design of the bearing surface layer, which solves the problems of uneven load distribution caused by axis inclination or installation errors, and the inability to effectively conduct and dissipate heat, thereby causing bearing overheating and affecting performance and safety. Especially in salt water environments, the limited bearings are easily corroded and have insufficient sound insulation performance, which cannot meet the current demand for a low-noise operating environment, thereby increasing the cost of bearing use.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions: a water-lubricated radial bearing based on a non-uniform thickness design of a pad surface layer, comprising:
[0007] A component mechanism is used for the purpose of reducing stress concentration, the component mechanism includes a bearing housing, a rotating shaft, and a lath assembly, the lath assembly is arranged inside the bearing housing, and the rotating shaft is arranged in the middle of the bearing housing, for jointly bearing and reducing the bearing load;
[0008] A locking mechanism is arranged inside the bearing housing and is used to quickly connect the slat assembly to the bearing housing, allowing flexible combination according to different application requirements and facilitating replacement and maintenance operations.
[0009] Preferably, the slat assembly includes a tile base and a tile surface layer, the tile base is fixedly connected to the inner side of the bearing housing, the tile surface layer is fixedly connected to the inner side of the tile base, a positioning block is fixedly connected to the outer side of the tile base, a positioning groove is opened in the middle of the bearing housing, and the positioning block is slidably connected in the middle of the positioning groove.
[0010] Preferably, the locking mechanism includes two compression springs 1, the adjacent ends of the two compression springs 1 are fixedly connected to a connecting plate, the adjacent sides of the two connecting plates are respectively fixedly connected to an electromagnet 1 and an electromagnet 2, the interior of the connecting plate is fixedly connected to a compression spring 2, the other end of the compression spring 2 is fixedly connected to an extrusion block, and the extrusion block is in contact with the positioning block.
[0011] Preferably, the tile surface layer and the tile base are both structures of non-uniform thickness, the thickness of the tile surface layer gradually increases along the axial direction, and the thickness of the tile base gradually decreases along the axial direction.
[0012] Preferably, the purpose of increasing the contact area between the inclined shaft and the tile surface layer is achieved by adjusting the thickness difference b-a of the tile surface layer. The thickness difference is related to the size and position of the eccentric load force, and the formula is: ba≈Ltanγ
[0013] Where L is the bearing length in m;
[0014] γ is the axis inclination angle, in degrees.
[0015] Preferably, when the tile surface layer is rubber, the tile surface layer is vulcanized on the inner surface of the tile base; when the tile surface layer is made of Sailong and Feilong polymer materials, the tile surface layer and the tile base are bonded with underwater super glue.
[0016] Preferably, the bearing adopts a combination of slat assemblies based on equal thickness tile surface layers and slat assemblies based on non-equal thickness tile surface layers to adapt to different application requirements. The combination methods include: the slat assemblies have the same circumferential angles and use non-equal thickness tile surface layers, and all slat assemblies have the same circumferential angles and use non-equal thickness tile surface layers at the bottom.
[0017] Preferably, another combination of bearings is that except for the bottom slat assembly which uses non-uniform thickness tile surface layers, the rest use slat assemblies with uniform thickness tile surface layers, and the circumferential angle of the bottom slat assembly is larger than the circumferential angles of the remaining slat assemblies.
[0018] Preferably, the bearing is installed in an application where the bearing is unbalancedly loaded due to the tilt of the propeller shaft of the ship's propulsion shaft system.
[0019] Preferably, the tile surface layer includes: a wear-resistant and elastic buffer layer, a heat dissipation and antistatic layer, and an anti-corrosion and sound insulation layer;
[0020] The wear-resistant and elastic buffer layer comprises the following components by weight percentage:
[0021] Ultra-high molecular weight polyethylene accounts for 75% to 85%;
[0022] Carbon nanotubes account for 10% to 20%;
[0023] Silica gel particles account for 3% to 7%;
[0024] The heat dissipation and antistatic layer includes the following components by weight percentage:
[0025] Graphite accounts for 70% to 80%;
[0026] Copper nanowires account for 15% to 25%;
[0027] High-impact polystyrene accounts for 3% to 7%;
[0028] The anti-corrosion and sound insulation layer includes the following components by weight percentage:
[0029] Porous polyurethane accounts for 80% to 90%;
[0030] The metal-organic framework powder accounts for 10% to 20%.
[0031] Working principle: When in use, by supplying power to electromagnet 1 and electromagnet 2, the relative electromagnet 1 and electromagnet 2 are moved away from each other, and at the same time, the two connecting plates are driven to compress the two compression springs 1. At this time, by inserting the bearing base into the bearing housing, when the positioning block passes over the original position of electromagnet 1 and electromagnet 2, the power supply state of electromagnet 1 and electromagnet 2 is disconnected, and under the action of compression spring 1, the two connecting plates can bring electromagnet 1 and electromagnet 2 closer to each other, thereby restricting the positioning block, so that the bearing base and the bearing housing are quickly connected. When the two connecting plates are close to each other, the positioning block will squeeze the extrusion block, so that the extrusion block compresses the compression spring 2. When the two connecting plates are in contact, the extrusion block can squeeze the positioning block under the action of compression spring 2, thereby further improving the stability of the bearing base;
[0032] Among them, when the load increases, the tile surface layer can be quickly replaced to increase the thickness of the tile surface layer, thereby reducing the problems of stress concentration and wear.
[0033] The present invention provides a water-lubricated radial bearing based on a non-uniform thickness design of a tile surface layer. It has the following beneficial effects:
[0034] 1. The present invention adopts a non-uniform thickness structure of the tile surface layer, so that the thickness of the tile surface layer gradually becomes thicker and the deformation gradually increases as the load increases, thereby achieving the purpose of increasing the contact area and reducing stress concentration. It can effectively solve the problems of the existing water-lubricated tail bearing tile surface adopting an equal thickness design, large local deformation, stress concentration and severe wear under the action of eccentric load.
[0035] 2. The present invention can accurately configure the material according to the specific needs of the application through the non-uniform thickness design of the tile surface layer, reducing material waste. At the same time, due to reduced wear and tear, the maintenance cycle is extended, further reducing maintenance costs.
[0036] 3. The present invention can use the locking mechanism to quickly replace the combination of equal-thickness slats and unequal-thickness slats of the tile surface layer and the circumferential angles of the unequal-thickness slats according to actual working conditions, thereby giving full play to the advantages of the unequal-thickness design and optimizing the bearing performance, while avoiding the problem of increased costs when all slats adopt a unequal-thickness structure.
[0037] 4. The present invention improves the adaptability of the bearing by improving the tile surface layer, so that the bearing can perform well under high humidity, high salt corrosion or extreme temperature conditions. At the same time, it increases the service life of the bearing, reduces the frequency of bearing replacement, and thus reduces the cost of bearing use. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 A perspective view of the present invention;
[0039] Figure 2 It is a structural schematic diagram of the composition mechanism of the present invention;
[0040] Figure 3 It is a structural schematic diagram of the locking mechanism of the present invention;
[0041] Figure 4 and Figure 5 It is a schematic diagram of the structure of the slats of different shapes and non-uniform thickness of the present invention;
[0042] Figure 6 and Figure 7 It is a structural schematic diagram of implementation mode 1 of the present invention;
[0043] Figure 8 and Fig. 9 This is a schematic diagram of the structure of Embodiment 2 of the present invention;
[0044] Fig.10 It is a structural schematic diagram of implementation mode 3 of the present invention.
[0045] Among them, 10, component mechanism; 101, tile surface layer; 102, tile base; 103, bearing housing; 104, positioning block; 105, positioning groove; 107, rotating shaft; 60, locking mechanism; 601, compression spring 1; 602, connecting plate; 603, electromagnet 1; 604, electromagnet 2; 605, compression spring 2; 606, extrusion block. DETAILED DESCRIPTION
[0046] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] Please refer to the attached Figure 1 -Attached Fig.10 The embodiment of the present invention provides a water-lubricated radial bearing based on a non-uniform thickness design of a pad surface layer, comprising:
[0048] The component mechanism 10 is used for the purpose of reducing stress concentration. The component mechanism 10 includes a bearing housing 103, a rotating shaft 107, and a slat assembly. The slat assembly is arranged inside the bearing housing 103. The rotating shaft 107 is arranged in the middle of the housing bearing housing 103 to share the load and reduce the bearing load. The bearing housing 103 is used to provide overall structural strength and protect internal components. The non-uniform thickness design of the slat assembly allows the contact area and pressure distribution to be automatically adjusted according to the load distribution when the rotating shaft 107 moves, effectively reducing stress concentration, thereby improving the bearing capacity and durability of the entire bearing, and extending the service life of the bearing.
[0049] The locking mechanism 60 is arranged inside the bearing housing 103 and is used to quickly connect the slat assembly to the bearing housing 103, allowing flexible combination according to different application requirements and facilitating replacement and maintenance operations. When the bearing needs to use slat assemblies of different thicknesses under different operating conditions, the locking mechanism 60 can quickly replace and reconfigure the slat assembly to adapt to the changing load.
[0050] Please refer to the attached Figure 1 -Attached Fig.10In a preferred embodiment of the present invention, the slat assembly includes a tile base 102 and a tile surface layer 101. The tile base 102 is fixedly connected to the inner side of the bearing housing 103, and the tile surface layer 101 is fixedly connected to the inner side of the tile base 102. A positioning block 104 is fixedly connected to the outer side of the tile base 102. A positioning groove 105 is opened in the middle of the bearing housing 103. The positioning block 104 is slidably connected to the middle of the positioning groove 105. The tile base 102 can provide a stable support platform for the tile surface layer 101. At the same time, the tile surface layer 101 is directly in contact with the rotating shaft 107 and is responsible for providing sliding lubrication function, wherein: a tile surface layer 101 and a tile base 102 form a slat assembly, and multiple slats are evenly arranged and fixed on the inner wall of the bearing housing 103 to jointly bear the bearing load.
[0051] Please refer to the attached Figure 2 and attached Figure 3 In a preferred embodiment of the present invention, the locking mechanism 60 includes two compression springs 1 601, and the adjacent ends of the two compression springs 1 601 are fixedly connected to a connecting plate 602, and the adjacent sides of the two connecting plates 602 are respectively fixedly connected to an electromagnet 1 603 and an electromagnet 2 604, and the interior of the connecting plate 602 is fixedly connected to a compression spring 2 605, and the other end of the compression spring 2 605 is fixedly connected to an extrusion block 606, and the extrusion block 606 is in contact with the positioning block 104. By activating the electromagnet 1 603 and the electromagnet 2 604, the activated electromagnet 1 603 and the electromagnet 2 604 push the two connecting plates 602 to compress the compression spring 1 601, thereby releasing the restriction on the positioning block 104. The tile base 102 and the tile surface layer 101 can be installed or removed. At the same time, after the tile base 102 and the tile surface layer 101 are connected, by canceling the activated electromagnet 1 603 and the electromagnet 2 604 and under the action of the compression spring 1 601, the connecting plate 602 can drive the electromagnet 1 603 and the electromagnet 2 604 to approach each other, thereby limiting the positioning block 104 and improving the installation efficiency of the tile base 102 and the tile surface layer 101. The positioning block 104 can be squeezed after the connection by the action of the compression spring 2 605 and the squeezing block 606, thereby further improving the stability of the tile base 102, improving the overall maintenance efficiency, and being able to be flexibly combined and configured according to different application requirements.
[0052] Please refer to the attached Figure 1 -Attached Fig.10 In a preferred embodiment of the present invention, the shoe surface layer 101 and the shoe base 102 are both non-uniform thickness structures. The thickness of the shoe surface layer 101 gradually increases along the axial direction, and the thickness of the shoe base 102 gradually decreases along the axial direction. Through the above-mentioned gradually thickening design, a larger contact area can be provided in areas with higher loads, effectively dispersing pressure, reducing wear and heat accumulation, and significantly improving the overall durability and operating life of the bearing by improving load distribution and optimizing lubrication conditions.
[0053] Please see attached Figure 1 -Attached Fig.10 In a preferred embodiment of the present invention, the purpose of increasing the contact area between the inclined shaft 107 and the tile surface layer 101 is achieved by adjusting the thickness difference b-a of the tile surface layer 101. The thickness difference is related to the size and position of the eccentric load force, and the formula is; ba≈Ltanγ
[0054] Where L is the bearing length in m;
[0055] γ is the axis inclination angle, measured in degrees. The thickness of the bearing surface layer 101 is adjusted to adapt to the inclination of the rotating shaft 107, thereby increasing the contact area and more effectively dispersing the eccentric load force caused by the inclination. The increased contact area reduces the contact stress, thereby reducing the wear rate and increasing the service life of the bearing, and enhancing the adaptability and stability of the bearing under different working conditions, especially in high-load and high-speed applications.
[0056] Please see attached Figure 1 -Attached Fig.10 In a preferred embodiment of the present invention, when the tile surface layer 101 is rubber, the tile surface layer 101 is vulcanized on the inner surface of the tile base 102; when the tile surface layer 101 is made of Sailong and Feilong polymer materials, the tile surface layer 101 and the tile base 102 are bonded with underwater super glue. The vulcanization process is a prior art, which mainly involves the rubber macromolecules reacting chemically with the cross-linking agent sulfur under heating, cross-linking to form a three-dimensional network structure, and bonding to the tile base 102. The vulcanized rubber has better wear resistance and elasticity, and is suitable for environments with large dynamic loads. When the tile surface layer 101 is made of polymer materials, the bonding technology can ensure that the tile surface layer 101 will not fall off even under high load or high-speed operation, and is suitable for underwater and other harsh environments. It can prevent the intrusion of water and other corrosive substances, and ensure the long-term stability and durability of the bearing under different environmental and operating conditions.
[0057] Please see attached Figure 1 -Attached Fig.10 When the bearing of the present invention is used, the thicker end of the tile surface layer 101 should be installed close to the propeller.
[0058] Please see attached Figure 1 -Attached Fig.10 The present invention adopts a combination of slats based on equal thickness tile surface layers and slats based on non-equal thickness tile surface layers to adapt to different application requirements. The combination methods include: all slat components have the same circumferential angle and use non-equal thickness tile surface layers; all slat components have the same circumferential angle and the bottom slat component uses non-equal thickness tile surface layers; except for the bottom slat component using non-equal thickness tile surface layers, other slat components all use equal thickness tile surface layers, and the circumferential angle of the bottom slat component is larger than the circumferential angles of other slat components.
[0059] Please refer to the attached Figure 1 -Attached Fig.10 In a preferred embodiment of the present invention, the bearing adopts a combination of a slat assembly based on an equal thickness tile surface layer and a slat assembly based on a non-equal thickness tile surface layer to adapt to different application requirements. The combination methods include: the slat assemblies have the same circumferential angle and use a non-equal thickness tile surface layer, and all the slat assemblies have the same circumferential angle and use a non-equal thickness tile surface layer at the bottom.
[0060] The specific combination is as follows:
[0061] Implementation method 1. Design of non-uniform thickness tile surface layer, as shown in the attached Figure 6 and attached Figure 7 As shown:
[0062] On the radial section of the shaft, all slat components adopt a non-uniform thickness tile surface layer design, which means that the thickness of each slat component varies along its length to adapt to different load distributions, which is suitable for occasions where the inclined shaft performs conical movement.
[0063] Embodiment 2. Combination of equal thickness and non-equal thickness strip assembly design; as shown in the attached Figure 8 and attached Fig. 9 As shown:
[0064] The upper part of the bearing adopts a tile surface layer of equal thickness, and the lower part adopts a tile surface layer of non-equal thickness. The design of the above-mentioned equal thickness slat assembly can provide uniform load-bearing capacity, and the design of the lower part using non-equal thickness slat assembly can resist continuous single-direction tilting pressure. By changing the thickness of the slats, the adaptability of the bearing to these loads can be optimized, thereby improving its overall stability and efficiency. It can not only provide the necessary structural support, but also reduce the overall weight, because the non-equal thickness slats can reduce material usage without sacrificing performance.
[0065] Implementation method 3. Bottom reinforcement non-uniform thickness design: as shown in the attached Fig.10 As shown:
[0066] Non-equal thickness slat assemblies are used in the bottom area of the bearing, and equal thickness slat assemblies are used in other areas. The circumferential angle of the bottom slat assembly is also larger than that of other slat assemblies. The non-equal thickness design of the bottom slat assembly not only provides a larger contact area, but also enhances the load-bearing capacity of the local area by changing the width or circumferential angle of the slat assembly, thereby improving the load-bearing capacity of the bearing. This design is particularly suitable for occasions where the bearing is subjected to eccentric loads or high dynamic loads.
[0067] Please refer to the attached Figure 1 -Attached Fig.10 In a preferred embodiment of the present invention, the tile surface layer 101 includes: a wear-resistant and elastic buffer layer, a heat dissipation and antistatic layer, and an anti-corrosion and sound insulation layer;
[0068] The wear-resistant and elastic buffer layer comprises the following components by weight percentage:
[0069] Ultra-high molecular weight polyethylene accounts for 75% to 85%;
[0070] Carbon nanotubes account for 10% to 20%;
[0071] Silica gel particles account for 3% to 7%;
[0072] The heat dissipation and antistatic layer includes the following components by weight percentage:
[0073] Graphite accounts for 70% to 80%;
[0074] Copper nanowires account for 15% to 25%;
[0075] High-impact polystyrene accounts for 3% to 7%;
[0076] The anti-corrosion and sound insulation layer includes the following components by weight percentage:
[0077] Porous polyurethane accounts for 80% to 90%;
[0078] The metal-organic framework powder accounts for 10% to 20%.
[0079] Example 1: Standard marine application
[0080] Wear-resistant and elastic buffer layer:
[0081] Material ratio:
[0082] Ultra-high molecular weight polyethylene: 80%
[0083] Carbon nanotubes: 15%
[0084] Silica gel particles: 5%
[0085] Preparation process:
[0086] The carbon nanotubes and silica particles are treated with acid and then mixed with ultra-high molecular weight polyethylene;
[0087] The mixture was mixed and extruded using a twin-screw extruder at 180°C.
[0088] The mixture is rolled into sheets with thickness gradually increasing from 0.5mm to 1.5mm
[0089] Heat dissipation and antistatic layer:
[0090] Material ratio:
[0091] Graphite: 75%
[0092] Copper nanowires: 20%
[0093] High impact polystyrene: 5%
[0094] Preparation process:
[0095] Graphite and copper nanowires were mixed using a ball mill in a liquid nitrogen environment to ensure uniform distribution;
[0096] The mixture was blended with high impact polystyrene at 150°C and then formed into a sheet by hot pressing.
[0097] Anti-corrosion and sound insulation layer:
[0098] Material ratio:
[0099] Porous polyurethane: 85%
[0100] Metal-organic framework powder: 15%
[0101] Preparation process:
[0102] The metal-organic framework powders were distributed in porous polyurethane using a solution impregnation method;
[0103] The metal-organic framework powders were fixed by freeze drying and then subjected to hot pressing to form the final layer.
[0104] Example 2: High temperature industrial application
[0105] Wear-resistant and elastic buffer layer:
[0106] Material ratio adjustment:
[0107] Ultra-high molecular weight polyethylene: 75%
[0108] Carbon nanotubes: 20%
[0109] Silica gel particles: 5%
[0110] Preparation process:
[0111] The surface functionalized carbon nanotubes are mixed with polyethylene using ultrasonic dispersion technology; the mixture is formed into a gradually thickening layered structure by high temperature hot pressing at 200°C.
[0112] Heat dissipation and antistatic layer:
[0113] Material ratio adjustment:
[0114] Graphite: 70%
[0115] Copper nanowires: 25%
[0116] High impact polystyrene: 5%
[0117] Preparation process:
[0118] Graphite and copper nanowires are uniformly mixed in high-impact polystyrene using a hot extrusion method; the mixture is formed by hot plate pressing to ensure the uniformity and strength of the heat dissipation layer.
[0119] Anti-corrosion and sound insulation layer:
[0120] Material ratio adjustment:
[0121] Porous polyurethane: 80%
[0122] Metal-organic framework powder: 20%
[0123] Preparation process:
[0124] The metal-organic framework powder is uniformly deposited on the polyurethane surface through chemical vapor deposition technology; it is cured at high temperature to ensure the integrity and durability of the layer.
[0125] Example 3: High Impact Application
[0126] Wear-resistant and elastic buffer layer:
[0127] Material ratio:
[0128] Ultra-high molecular weight polyethylene: 85%
[0129] Carbon nanotubes: 10%
[0130] Silica gel particles: 5%
[0131] Preparation process:
[0132] The carbon nanotubes and silica particles are pre-surface treated in a vacuum environment to increase their compatibility in polyethylene;
[0133] The wear-resistant layer is produced by high-pressure extrusion technology, ensuring uniform mass distribution, and is formed by hot pressing.
[0134] Heat dissipation and antistatic layer:
[0135] Material ratio:
[0136] Graphite: 80%
[0137] Copper nanowires: 15%
[0138] High impact polystyrene: 5%
[0139] Preparation process:
[0140] Graphite and copper nanowires were subjected to high-energy ball milling under vacuum to improve their dispersion in polystyrene;
[0141] The mixture is thermoformed to form a layer with excellent heat dissipation and antistatic properties.
[0142] Anti-corrosion and sound insulation layer:
[0143] Material ratio:
[0144] Porous polyurethane: 90%
[0145] Metal-organic framework powder: 10%
[0146] Preparation process:
[0147] The metal-organic framework powder was evenly distributed in polyurethane using an ultrasonic-assisted solvent impregnation method;
[0148] Low temperature curing and heat treatment ensure the stability and functionality of the sound insulation and anti-corrosion layers.
[0149] Example 4: Low temperature marine applications
[0150] Wear-resistant and elastic buffer layer:
[0151] Material ratio:
[0152] Ultra-high molecular weight polyethylene: 85%
[0153] Carbon nanotubes: 10%
[0154] Silica gel particles: 5%
[0155] Preparation process:
[0156] Through cold treatment technology, carbon nanotubes and silica particles are pre-treated to improve their bonding with polyethylene;
[0157] Mixing and calendering are carried out at low temperatures to prevent thermal degradation of the material, and the desired layered structure is formed by cold pressing technology.
[0158] Heat dissipation and antistatic layer:
[0159] Material ratio:
[0160] Graphite: 75%
[0161] Copper nanowires: 20%
[0162] High impact polystyrene: 5%
[0163] Preparation process:
[0164] Copper nanowires and graphite nanoparticles were uniformly mixed in high-impact polystyrene using electrospinning technology under low temperature conditions;
[0165] Through cold pressing technology, the uniformity and structural integrity of the heat dissipation layer are ensured.
[0166] Anti-corrosion and sound insulation layer:
[0167] Material ratio:
[0168] Porous polyurethane: 85%
[0169] Metal-organic framework powder: 15%
[0170] Preparation process:
[0171] The metal-organic framework powder was uniformly distributed in porous polyurethane using liquid deposition at low temperature to maintain the chemical stability and structural integrity of the material;
[0172] Cold curing technology is used to ensure the functionality of the sound insulation and anti-corrosion layers.
[0173] Example 5: High-speed motion application
[0174] Wear-resistant and elastic buffer layer:
[0175] Material ratio:
[0176] Ultra-high molecular weight polyethylene: 75%
[0177] Carbon nanotubes: 15%
[0178] Silica gel particles: 10%
[0179] Preparation process:
[0180] Premixing carbon nanotubes and silica particles in a high-energy mixer to improve their dispersion in ultra-high molecular weight polyethylene;
[0181] Through high-speed extrusion and hot pressing technology, the uniformity and durability of the wear-resistant layer are ensured.
[0182] Heat dissipation and antistatic layer:
[0183] Material ratio:
[0184] Graphite: 80%
[0185] Copper nanowires: 15%
[0186] High impact polystyrene: 5%
[0187] Preparation process:
[0188] High shear mixing technology was used to ensure uniform distribution of graphite and copper nanowires in high-impact polystyrene;
[0189] Through high-pressure hot pressing, a layer with excellent heat dissipation and antistatic properties is formed.
[0190] Anti-corrosion and sound insulation layer:
[0191] Material ratio:
[0192] Porous polyurethane: 90%
[0193] Metal-organic framework powder: 10%
[0194] Preparation process:
[0195] The metal-organic framework powder was evenly distributed in the porous polyurethane by high-pressure spraying technology;
[0196] Rapid curing technology ensures the stability and functionality of the sound insulation and anti-corrosion layers.
[0197] Comparative Example 1:
[0198] The difference from Example 1 is that Comparative Example 1 uses conventional polyethylene instead of ultra-high molecular weight polyethylene, and does not add carbon nanotubes and silica gel particles. The remaining preparation steps are the same as those of the present invention.
[0199] Comparative Example 2:
[0200] The difference from Example 2 is that in Comparative Example 2, the heat dissipation and antistatic layer uses only graphite, and does not use a mixture of copper nanowires and high-impact polystyrene, and the remaining preparation steps are the same as those of the present invention.
[0201] Comparative Example 3:
[0202] The difference from Example 3 is that in Example 3, carbon nanotubes without any functionalization treatment are used in the wear-resistant and elastic buffer layer, resulting in poor dispersion of the carbon nanotubes in the polyethylene matrix. The remaining preparation steps are the same as those of the present invention.
[0203] Comparative Example 4:
[0204] The difference from Example 4 is that Comparative Example 4 uses ethylenediaminetetraacetic acid commonly used on the market as a metal complexing agent instead of using metal-organic framework powder, and the remaining preparation steps are the same as those of the present invention.
[0205] Comparative Example 5:
[0206] The difference from Example 5 is that in Comparative Example 5, the anti-corrosion and sound insulation layer only uses conventional porous polyurethane without adding metal-organic framework powder, and the remaining preparation steps are the same as those of the present invention.
[0207] Experiment 1: Wear resistance test
[0208] Purpose: To test and compare the wear rates of the wear-resistant and elastic buffer layer provided by the present invention and conventional wear-resistant materials under standardized conditions, so as to evaluate and verify the improvement in the wear resistance of the material of the present invention.
[0209] Experimental Materials:
[0210] Example sample: A composite material containing 80% ultra-high molecular weight polyethylene, 15% carbon nanotubes, and 5% silica gel particles.
[0211] Comparison sample: 100% conventional polyethylene.
[0212] Experimental equipment:
[0213] Dry sand rubber wheel wear tester
[0214] Standard sandpaper
[0215] Electronic balance
[0216] Experimental setup:
[0217] Both materials were processed into test pieces with a size of 10cmx10cmx0.5cm;
[0218] Make sure the surface is flat and has no obvious defects.
[0219] Wear test machine settings:
[0220] Load standard sandpaper onto the wear wheel of the testing machine;
[0221] Adjust the sandpaper to ensure that the contact area with the test piece is uniform.
[0222] Experimental steps:
[0223] Weight record:
[0224] Use an electronic balance to measure and record the initial weight of each test piece.
[0225] Wear test:
[0226] Fix the sample on the sample holder of the wear tester;
[0227] Set the wear wheel speed to 200RPM and the wear time to 10 minutes;
[0228] Ensure that the test piece is in even contact with the sandpaper during the abrasion process.
[0229] Weight Measurement:
[0230] After the test is completed, remove all impurities from the sample;
[0231] The weight of each sample was again measured using an electronic balance.
[0232] Data recording and analysis:
[0233] Calculate the wear volume of each sample;
[0234] The wear resistance of the example samples and the comparative samples was evaluated by comparing the wear amount difference.
[0235] The experimental results are shown in Table 1:
[0236] Table 1 Comparison of wear resistance test results
[0237] Sample Type Test No. Initial weight (g) Final weight (g) Wear amount (g) Example 1 50 49.78 0.22 Example 2 50.01 49.8 0.21 Comparison samples 1 50 49.65 0.35 Comparison samples 2 50.02 49.68 0.34
[0238] From the data in Table 1, it can be seen that the example samples show lower wear than the control samples, which indicates that the added carbon nanotubes and silica gel particles effectively improve the wear resistance of the material.
[0239] Experiment 2: Heat dissipation performance test
[0240] Purpose: To compare the heat dissipation performance of the heat dissipation and antistatic layer of the present invention with that of the traditional graphite heat dissipation layer.
[0241] Experimental Materials:
[0242] Example sample: graphite 75%, copper nanowire 20%, high impact polystyrene 5%.
[0243] Comparison sample: Pure graphite 100%.
[0244] Experimental equipment:
[0245] Laser flash device
[0246] Temperature controlled hot plate
[0247] Thermocouple
[0248] Data Logger
[0249] Experimental setup:
[0250] Prepare two sets of sample plates, three pieces in each set, with the size of 5cmx 5cmx0.5cm;
[0251] Each sample is evenly coated with thermal conductive paste to ensure good heat transfer.
[0252] Experimental steps:
[0253] Sample pretreatment:
[0254] All sample surfaces were cleaned and evenly coated with thermal conductive paste.
[0255] Device settings:
[0256] Place the sample on a temperature-controlled hot stage, set the temperature of the hot stage to 50°C, and maintain a constant temperature.
[0257] To activate the laser flash device:
[0258] Laser flash thermal conductivity test was performed on each sample, and the required time and temperature change were recorded.
[0259] Real-time temperature monitoring:
[0260] Use a thermocouple to measure the surface temperature of the sample, record it every 30 seconds, and record it continuously for 10 minutes. Data recording:
[0261] The temperature change and time data were entered into a data logger for subsequent analysis.
[0262] Repeat the test:
[0263] The samples of each material were tested three times to ensure the reliability and repeatability of the results. The experimental results are shown in Table 2:
[0264] Table 2 Heat dissipation performance test results
[0265]
[0266] From the data in Table 2, it can be seen that the difference in heat dissipation performance between the example sample and the comparative sample under the same test conditions is shown. The expected results show that the composite material with copper nanowires added has better thermal conductivity and lower final temperature, showing improved heat dissipation performance.
[0267] Experiment 3: Antistatic performance test
[0268] Objective: To evaluate the effect of adding copper nanowires to the heat dissipation and antistatic layer of the present invention on the antistatic performance and compare it with the traditional graphite layer without copper nanowires added
[0269] Experimental Materials:
[0270] Example sample: graphite 75%, copper nanowire 20%, high impact polystyrene 5%.
[0271] Comparison sample: Pure graphite 100%.
[0272] Experimental equipment:
[0273] Resistivity test device
[0274] Static Voltage Tester
[0275] Environmental control room
[0276] Experimental setup:
[0277] Prepare rectangular samples, each sample size is 10cmx10cm;
[0278] All samples were tested in an environmentally controlled room to eliminate interference from environmental factors.
[0279] Experimental steps:
[0280] Sample preparation:
[0281] Clean all samples to ensure that there is no dust or other impurities on the surface.
[0282] Environment settings:
[0283] The temperature of the environmental control room was set to 25 °C and the relative humidity to 50% to keep the conditions consistent throughout the experiment.
[0284] Resistivity test:
[0285] Use a resistivity test device to test the surface resistivity of each sample in accordance with ASTM D257 standard;
[0286] The resistance value of each sample was recorded.
[0287] Electrostatic voltage test:
[0288] Use an electrostatic voltage tester to measure the electrostatic voltage of the sample after friction;
[0289] Record the voltage change before and after friction.
[0290] Data recording and analysis:
[0291] All test data are recorded and analyzed to evaluate the antistatic performance.
[0292] The experimental results are shown in Table 3:
[0293] Table 3 Antistatic performance test results
[0294] Sample Type Test No. Measurement environment Surface resistivity(Ω) Static voltage (V) Example 1 25℃,50%RH <![CDATA[1.5x10 5 ]]> 100 Example 2 25℃,50%RH <![CDATA[1.8x10 5 ]]> 90 Example 3 25℃,50%RH <![CDATA[1.6x10 5 ]]> 95 Comparison samples 1 25℃,50%RH <![CDATA[5.0x10 7 ]]> 500 Comparison samples 2 25℃,50%RH <![CDATA[4.8x10 7 ]]> 480 Comparison samples 3 25℃,50%RH <![CDATA[4.9x10 7 ]]> 490
[0295] From the data in Table 3, it can be observed that the example sample has significantly lower surface resistivity and electrostatic voltage than the comparative sample, showing its excellent antistatic performance. The results of this experiment will help verify that the addition of copper nanowires can significantly improve the antistatic performance of the material, thereby reducing the risk of static electricity accumulation, which is particularly important for sensitive applications such as electronic devices.
[0296] Experiment 4: Anti-corrosion performance test
[0297] Objective: To evaluate the anti-corrosion performance of the anti-corrosion and sound-insulating layer of the present invention and that of conventional porous polyurethane materials, in order to verify the improved effect of the material of the present invention.
[0298] Experimental Materials:
[0299] Example sample: porous polyurethane 85%, metal-organic framework powder 15%.
[0300] Comparison sample: Pure porous polyurethane 100%.
[0301] Experimental equipment:
[0302] Salt spray test chamber
[0303] Corrosion assessment tools include optical microscope and corrosion depth gauge
[0304] Environmental control equipment to maintain constant temperature and humidity
[0305] Experimental setup:
[0306] Prepare rectangular samples, each sample size is 10cmx10cmx0.5cm;
[0307] Ensure that all sample surfaces are clean and free of grease.
[0308] Experimental steps:
[0309] Sample preparation:
[0310] All samples were cleaned to remove surface contaminants.
[0311] Salt spray test chamber settings:
[0312] Set the temperature of the salt spray test chamber to 35 °C, relative humidity to 100%, and use 5% saline solution.
[0313] Test execution:
[0314] Place the specimen in a salt spray test chamber;
[0315] Exposure continued for 72 hours, during which changes in the specimen's appearance were recorded regularly.
[0316] Post-evaluation:
[0317] After the test, remove the sample, rinse with clean water and dry;
[0318] Use an optical microscope to observe surface corrosion;
[0319] Use a corrosion depth gauge to measure the size of any corrosion pits.
[0320] Data recording and analysis:
[0321] The corrosion conditions of all samples were recorded and analyzed, and the performance differences between the example samples and the comparative samples were compared.
[0322] The experimental results are shown in Table 4:
[0323] Table 4 Salt spray corrosion test results
[0324]
[0325] From the data in Table 4, it can be seen that the example samples have significant advantages over the comparative samples in terms of corrosion resistance. By comparing the corrosion degree and the depth of the corrosion pits, it can be clearly seen that the addition of the metal-organic framework of the present invention significantly improves the corrosion resistance of the material, thereby confirming the innovation and effectiveness of the present invention in improving the material's resistance to environmental influences.
[0326] Experiment 5: Sound insulation test
[0327] Objective: To evaluate the acoustic performance of the anti-corrosion and sound insulation layer of the present invention compared with conventional porous polyurethane materials, especially in terms of sound absorption and sound insulation.
[0328] Experimental Materials:
[0329] Example sample: porous polyurethane 85%, metal-organic framework powder 15%.
[0330] Comparison sample: Pure porous polyurethane 100%.
[0331] Experimental equipment:
[0332] Echo Chamber
[0333] Sound pressure level meter
[0334] Frequency Analyzer
[0335] Environmental noise control system
[0336] Experimental setup:
[0337] Prepare flat samples, each sample size is 50cmx50cmx5cm;
[0338] Ensure that all samples reach the same acclimatization conditions, such as temperature and humidity, before testing.
[0339] Experimental steps:
[0340] Sample preparation:
[0341] Make sure the sample surface is clean and free of dust or other impurities.
[0342] Echo Chamber Preparation:
[0343] The echo chamber temperature and humidity were adjusted to standard test conditions: 23°C and 50% relative humidity.
[0344] Install the sample:
[0345] Fix the sample in the test position in the echo chamber to ensure that the sample is fully exposed to the test environment.
[0346] Sound Test:
[0347] Using a sound pressure level meter, measure the sound pressure level of the sample from a number of different points;
[0348] The sound absorption and reflection data at specific frequencies are recorded by a frequency analyzer.
[0349] Data Records:
[0350] Throughout the test, data was continuously recorded to ensure reliability and accuracy;
[0351] Record the minimum and maximum absorbance and the corresponding frequencies.
[0352] The experimental results are shown in Table 5:
[0353] Table 5 Sound absorption and sound insulation test results
[0354] Sample Type Test No. Test frequency (Hz) Sound pressure level (dB) Absorption rate (%) Example 1 250 30 85 Example 2 500 28 82 Example 3 1000 25 90 Comparison samples 1 250 40 55 Comparison samples 2 500 38 58 Comparison samples 3 1000 35 60
[0355] From the data in Table 5, it can be obtained that: the above table records the sound pressure level and sound absorption rate at different frequencies, showing that the example samples have significantly improved sound insulation and sound absorption performance compared to the comparative samples. The example samples show lower sound pressure levels and higher absorption rates, especially in the high-frequency range, which proves that the addition of metal-organic framework powder can significantly improve acoustic performance and provide a better material choice for sensitive environments such as libraries, conference rooms, etc.
[0356] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A water-lubricated radial bearing based on a non-uniform thickness design of the pad surface layer, characterized in that: include: A component mechanism (10) is used for the purpose of reducing stress concentration, the component mechanism (10) comprising a bearing housing (103), a rotating shaft (107), and a slat assembly, the slat assembly is arranged inside the bearing housing (103), the rotating shaft (107) is arranged in the middle of the bearing housing (103), and is used to share the load to reduce the bearing load; A locking mechanism (60) is arranged inside the bearing housing (103) and is used to quickly connect the slat assembly to the bearing housing (103), allowing flexible combination according to different application requirements and facilitating replacement and maintenance operations.
2. A water-lubricated radial bearing based on a non-uniform thickness design of a pad surface layer according to claim 1, characterized in that: The slat assembly comprises a tile base (102) and a tile surface layer (101); the tile base (102) is fixedly connected to the inner side of the bearing housing (103); the tile surface layer (101) is fixedly connected to the inner side of the tile base (102); a positioning block (104) is fixedly connected to the outer side of the tile base (102); a positioning groove (105) is provided in the middle of the bearing housing (103); and the positioning block (104) is slidably connected to the middle of the positioning groove (105).
3. The water-lubricated radial bearing based on the non-uniform thickness design of the pad surface layer according to claim 2 is characterized in that: The locking mechanism (60) comprises two compression springs (601), the adjacent ends of the two compression springs (601) are fixedly connected to a connecting plate (602), the adjacent sides of the two connecting plates (602) are respectively fixedly connected to an electromagnet (603) and an electromagnet (604), the interior of the connecting plate (602) is fixedly connected to a compression spring (605), the other end of the compression spring (605) is fixedly connected to an extrusion block (606), and the extrusion block (606) is in contact with the positioning block (104).
4. The water-lubricated radial bearing based on the non-uniform thickness design of the pad surface layer according to claim 2 is characterized in that: The tile surface layer (101) and the tile base (102) are both structures of non-uniform thickness. The thickness of the tile surface layer (101) gradually increases along the axial direction, while the thickness of the tile base (102) gradually decreases along the axial direction.
5. The water-lubricated radial bearing based on the non-uniform thickness design of the pad surface layer according to claim 2 is characterized in that: The purpose of increasing the contact area between the inclined rotating shaft (107) and the tile surface layer (101) is achieved by adjusting the thickness difference b-a of the tile surface layer (101). The thickness difference is related to the magnitude and position of the eccentric load force, and the formula is: ba≈Ltanγ Where L is the bearing length in m; γ is the axis inclination angle, in degrees.
6. The water-lubricated radial bearing based on the non-uniform thickness design of the pad surface layer according to claim 2 is characterized in that: When the tile surface layer (101) is rubber, the tile surface layer (101) is vulcanized on the inner surface of the tile base (102); when the tile surface layer (101) is made of Sailong and Feilong polymer materials, the tile surface layer (101) and the tile base (102) are bonded together using underwater strong glue.
7. The water-lubricated radial bearing based on the non-uniform thickness design of the pad surface layer according to claim 2 is characterized in that: The bearing adopts a combination of a slat assembly based on an equal thickness tile surface layer (101) and a slat assembly based on a non-equal thickness tile surface layer (101) to adapt to different application requirements. The combination method includes: the slat assemblies have the same circumferential angle and use a non-equal thickness tile surface layer (101), and all the slat assemblies have the same circumferential angle and use a non-equal thickness tile surface layer (101) at the bottom.
8. The water-lubricated radial bearing based on the non-uniform thickness design of the pad surface layer according to claim 2 is characterized in that: Another bearing assembly method is that except for the bottom slat assembly with non-uniform thickness tile surface layer (101), the rest all use slat assemblies with uniform thickness tile surface layer (101), and the circumferential angle of the bottom slat assembly is larger than the circumferential angles of the remaining slat assemblies.
9. The water-lubricated radial bearing based on the non-uniform thickness design of the pad surface layer according to claim 1 is characterized in that: The bearing is installed in an application where the bearing is unevenly loaded due to the inclination of the propeller shaft of the ship's propulsion shaft system.
10. The water-lubricated radial bearing based on the non-uniform thickness design of the pad surface layer according to claim 1, characterized in that: The tile surface layer (101) comprises: a wear-resistant and elastic buffer layer, a heat dissipation and antistatic layer, and an anti-corrosion and sound insulation layer; The wear-resistant and elastic buffer layer comprises the following components by weight percentage: Ultra-high molecular weight polyethylene accounts for 75% to 85%; Carbon nanotubes account for 10% to 20%; Silica gel particles account for 3% to 7%; The heat dissipation and antistatic layer includes the following components by weight percentage: Graphite accounts for 70% to 80%; Copper nanowires account for 15% to 25%; High-impact polystyrene accounts for 3% to 7%; The anti-corrosion and sound insulation layer includes the following components by weight percentage: Porous polyurethane accounts for 80% to 90%; The metal-organic framework powder accounts for 10% to 20%.
Citation Information
Patent Citations
Water-lubrication radial bearing designed based on unequal-thickness bush face layers
CN105864297A
Self-compensation quick-replacement water lubrication bearing
CN109505868A
Engine connecting rod connecting installation structure
CN210889697U
Novel PEEK high-performance sliding bearing
CN214888341U
Wear-resistant arc piece convenient to install
CN216430282U
Cited By
Batten type water lubricated bearing and assembling method thereof
CN121251692A
Magnetic composite water-lubricated rubber bearing with shock resistance
CN121828330A