Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction for hydrogen detection as well as preparation method and application of Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction

By loading Pd nanoparticles in one-dimensional WO3-SnO2 nanowire structure, the Galvanic replacement reaction is used to improve the sensitivity and stability of the hydrogen sensor, and the problems of low sensitivity and high working temperature of the existing hydrogen sensor are solved, achieving low cost and high efficiency hydrogen detection.

CN119044255APending Publication Date: 2024-11-29ZHENGZHOU UNIVERSITY OF LIGHT INDUSTRY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411158724.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing hydrogen sensors have the disadvantages of low sensitivity, high operating temperature and poor stability, making it difficult to achieve low cost, high sensitivity and excellent stability detection.

Method used

The Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction was synthesized by liquid phase reduction method. By loading Pd nanoparticles in the one-dimensional WO3-SnO2 nanowire structure, the active site and grain boundary contact interface of the material were improved by using Galvanic substitution reaction. , form a high-efficiency hydrogen sensor.

Benefits of technology

It realizes high sensitivity detection to hydrogen, reduces the working temperature to 90°C, and has good stability and low preparation cost, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044255A_ABST
    Figure CN119044255A_ABST
Patent Text Reader

Abstract

The invention discloses a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction for detecting hydrogen as well as a preparation method and application thereof.The nanowire is successfully synthesized through a liquid phase reduction method, organic acid and a tin compound are dissolved in a mixed solvent, and a stannate precursor is obtained under stirring at the room temperature; stirring the precursor and a tungsten compound in an organic solvent, performing centrifugal drying to obtain a sample, performing thermal reduction on the sample in an air atmosphere to obtain a one-dimensional WO3-SnO2 nanowire heterojunction, and finally attaching palladium particles to the one-dimensional WO3-SnO2 nanowire heterojunction under the action of a reducing agent to obtain the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction. According to the prepared sample, selectivity and stability to hydrogen are improved, good selectivity and excellent stability to hydrogen are achieved when the working temperature is 90 DEG C, and the sensitivity to 50 ppm hydrogen reaches 235.52.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction and application of the heterojunction as a hydrogen sensor. Background Art

[0002] Against the backdrop of the decreasing reserves of fossil fuels, air pollution and global warming, hydrogen, as a new type of clean energy, has attracted widespread attention and research. As a renewable, zero-carbon emission secondary energy carrier, hydrogen plays a vital role in ensuring energy supply security and promoting the achievement of carbon reduction targets. However, hydrogen molecules are very small and are prone to leakage during production, storage, transportation and use. In addition, the ignition point of hydrogen is only 585°C, and the content in the air is in the range of 4% to 75%. It will explode when exposed to open flames. Therefore, accurate and quantitative detection of hydrogen is of great significance.

[0003] At present, hydrogen sensors based on thermal conductivity, electrochemistry, catalysis, optics, acoustics and gas chromatography have been developed. Among them, metal oxide semiconductor (MOS) hydrogen sensors have attracted much attention due to their outstanding advantages such as excellent sensing performance, small scale and high integration. In addition, the construction of metal oxide heterostructures is also considered to be one of the most effective methods to improve gas sensing performance. This is because the different Fermi levels between different components are conducive to charge transfer, which can effectively increase the carrier density, thereby further improving gas sensing performance.

[0004] The literature reports that Pd / SnS2 / SnO2 nanocomposites were prepared by hydrothermal / impregnation method (Sensor. Actuat. B-Chem., 359, 2022, 131612). The optimal operating temperature of the prepared sensor for hydrogen response was too high and the stability effect was poor. The literature reports that Pd / SnO2 / PI nanocomposites were prepared by atomic layer deposition and cluster beam deposition technology (Advanced Electronic Materials, 9, 2023, 201047). The ALD ultra-thin oxide film was combined with CBD metal nanoparticles to prepare a hydrogen sensor with good selectivity and low detection limit, but the operating temperature was high and the sensitivity was low.

[0005] Existing hydrogen sensors still have disadvantages such as complicated preparation methods, high operating temperature, poor stability, and low sensitivity. Therefore, it is necessary to develop a hydrogen sensor with low operating temperature, high sensitivity, excellent stability, and low cost. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction with high sensitivity, low power consumption and excellent selectivity for hydrogen, and its application as a hydrogen sensor, in view of the shortcomings of hydrogen sensors such as low sensitivity, high operating temperature and poor stability.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions: The Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of the invention is synthesized by a liquid phase reduction method, wherein WO3 and SnO2 are in the same one-dimensional nanowire structure, and Pd nanoparticles are loaded on the surface of the one-dimensional WO3-SnO2 heterojunction carrier.

[0008] The present invention also provides a preparation method of a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction: first, an organic acid, a tin compound, and deionized water are added to a mixed solution of an organic solvent, a precipitate is removed by ultrasonication, stirring is continued at room temperature, and then a precursor is obtained by centrifugal washing and drying; then the precursor, an organic matter, and a tungsten compound are dissolved in an organic solvent, reacted under nitrogen protection under heating and stirring conditions, and the sample obtained by centrifugal washing and drying is calcined under high temperature conditions to obtain a one-dimensional WO3-SnO2 nanowire heterojunction; then the one-dimensional WO3-SnO2 nanowire, a palladium compound, and a reducing agent are dissolved in deionized water, ultrasonically dissolved and stirred, and a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction is obtained after centrifugal washing and drying. Specifically, the following steps are included: (1) Preparing a precursor: adding an organic acid, a tin compound and deionized water to a mixed solution of an organic solvent, ultrasonically removing a precipitate, continuing to stir at room temperature, and then centrifugally washing and drying to obtain a precursor; (2) Preparation of one-dimensional WO3-SnO2 nanowire heterojunction: The precursor, organic matter and tungsten compound prepared in step (1) are dissolved in an organic solvent to obtain a mixed solution A, reacted under nitrogen protection under heating and stirring conditions, centrifuged for washing and dried, and the obtained sample is calcined under high temperature conditions to obtain a one-dimensional WO3-SnO2 nanowire heterojunction; (3) Preparation of Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction: The one-dimensional WO3-SnO2 nanowire heterojunction prepared in step (2), a palladium compound, and a reducing agent are dissolved in deionized water, ultrasonically dissolved and stirred to obtain a mixed solution B, and centrifugally washed and dried to obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0009] Furthermore, the tin compound in step (1) is one or more of stannous chloride, stannous oxalate, stannous nitrate, and stannous bromide; the organic acid is one or more of oxalic acid, glycolic acid, and aminosulfonic acid; and the organic solvent is at least two of ethanol, propanol, glycerol, tetrahydrofuran, and n-hexane. Furthermore, in step (1), the mass ratio of the tin compound to the organic acid is 1:5 to 1:20.

[0010] Furthermore, the organic matter in step (2) is one or more of urea, polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, and sodium bis(2-ethylhexyl) succinate sulfonate; the tungsten compound is Na2WO4·2H2O, K2WO4, (NH4)6H2W 12 O 40 ·xH2O, H4[Si(W3O 10 )4]·xH2O, WCl6 or more.

[0011] Furthermore, the mass ratio of the precursor to the tungsten compound in step (2) is 1:0.02 to 1:0.2; and the total concentration of the precursor and the tungsten compound in the mixed solution A is 1 mg / mL to 3 mg / mL.

[0012] Furthermore, in step (2), the stirring heating temperature is 50-150°C, the nitrogen flow rate is 40-100 mL / min, and the stirring reaction time is 24-48 h; the calcination temperature is 400-800°C, the heating rate is 1°C / min-5°C / min, and the calcination time is 2-3 h.

[0013] Furthermore, the drying temperature in steps (1) to (3) is 60-100° C., and the drying time is 4-12 hours.

[0014] Furthermore, the palladium compound in step (3) is one or more of palladium acetate, palladium chloride, potassium palladate, and palladium nitrate; and the reducing agent is one or more of sodium borohydride, ascorbic acid, sodium hypophosphite, and citric acid.

[0015] Furthermore, the mass ratio of the reducing agent to the palladium compound in step (3) is 1:0.05 to 1:0.5; the mass ratio of the one-dimensional WO3-SnO2 nanowires to the palladium compound is 1:0.005 to 1:0.02; and the total concentration of the one-dimensional WO3-SnO2 nanowires and the palladium compound in the mixed solution B is 1 mg / mL to 10 mg / mL.

[0016] The typical preparation method of the present invention is as follows: (1) Preparation of precursor: dissolve the organic acid in a mixed solution of an organic solvent, stir to dissolve, then add the tin compound and deionized water to the mixed solution, ultrasonicate to remove the precipitate, continue stirring at room temperature, then wash away impurities with ethanol, and dry in an oven to obtain the precursor.

[0017] (2) Preparation of one-dimensional WO3-SnO2 nanowire heterojunction: The precursor prepared in step (1) is dissolved in ethanol, ultrasonically dissolved, and then an organic compound is added and stirred to dissolve. Finally, a tungsten compound is added, heated and stirred, and reacted under nitrogen protection. The sample is centrifuged, washed, and dried to obtain a sample, and then calcined under high temperature conditions to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0018] (3) Preparation of Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction: Dissolve the one-dimensional WO3-SnO2 nanowire prepared in step (2) in deionized water, stir to dissolve, add palladium compound, continue stirring, then add reducing agent, continue stirring, finally wash away impurities with deionized water and ethanol, and dry in an oven to obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0019] The present invention also provides the application of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction as a gas sensor in a high-sensitivity hydrogen sensor. When the operating temperature is 90°C, the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction as a gas sensor has good selectivity for hydrogen, and the sensitivity to 50 ppm hydrogen reaches 235.52.

[0020] The key to the innovation of the present invention is to prepare a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction. There are many methods for preparing materials for hydrogen sensors, but these methods are relatively cumbersome, and the prepared hydrogen sensors have high operating temperatures, poor stability and low sensitivity. The WO3-SnO2 heterojunction of the present invention is a one-dimensional nanowire heterostructure, and its two heterogeneous components are in the same one-dimensional structure. Therefore, more lattice stress and coordination unsaturated sites are generated at the grain boundary contact interface of the two components compared to the traditional out-of-plane heterostructure, and this site becomes an active site for the gas sensing process, providing an active site for activating the target hydrogen and oxygen. This novel structure helps to improve the operating temperature and sensitivity of oxide-type semiconductor hydrogen sensors.

[0021] The beneficial effect of the present invention is that the present invention composites Pd nanoparticles on the basis of a one-dimensional WO3-SnO2 nanowire heterojunction. The present invention is based on the Galvanic replacement reaction, and according to the difference in the redox potential of different metal ions in the solution, an ion replacement reaction is carried out under specific conditions to synthesize a one-dimensional WO3-SnO2 nanowire heterostructure. Since the structure is synthesized by an in situ replacement process, the two components WO3 and SnO2 are in the same one-dimensional nanowire structure. Compared with the traditional heterostructure, the structure has more surface coordinated unsaturated atoms and grain boundaries, and has more active sites, so it is beneficial to improve the sensitivity and selectivity to hydrogen, and has good stability; the sensitivity to 50 ppm hydrogen at a working temperature of 90°C reaches 235.52, and the working temperature is lower than that of the existing hydrogen sensor. The synthesis method of the present invention is innovative and has a low preparation cost; the morphology and size of the material are uniform; the response to hydrogen is high, and it is easy to realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 This is the XRD pattern of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction prepared in Example 6.

[0024] Figure 2 This is a scanning electron microscope (SEM) image of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction prepared in Example 6.

[0025] Figure 3 It is the response value of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction prepared in Example 6 to 50 ppm hydrogen at 70-130°C.

[0026] Figure 4 This is a long-term stability test of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction prepared in Example 6 to 50 ppm hydrogen within 30 days. DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with specific examples. It should be understood that the following examples are only used to illustrate the present invention and are not used to limit the scope of the present invention, and those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the above invention.

[0028] Example 1 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of this embodiment is as follows: (1) Dissolve 0.84 g oxalic acid in a mixed solution (9 mL ethanol + 51 mL propanol) and stir for 30 min to form a uniform, stable, clear and transparent solution. Then add 0.14 g stannous chloride and 3 mL H2O to the mixed solution. Ultrasonicate for 10 min to produce a precipitate. Continue stirring at room temperature for 3 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0029] (2) Dissolve 40 mg of the precursor prepared in (1) in 20 mL of ethanol, dissolve by ultrasonication and stir for 20 min, then add 10 mg of polyvinyl pyrrolidone and stir for 20 min, and finally add 4 mg of H4[Si(W3O 10 )4]·xH2O, stirred at 50 ℃ under nitrogen (nitrogen flow rate: 50 mL / min) for 24 h, washed with ethanol three times, and dried in an oven at 60 ℃ for 6 h to obtain a sample, which was placed in a tubular furnace and heated to 500 ℃ at a heating rate of 5 ℃ / min and kept warm for 3 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0030] (3) Dissolve 100 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 1 mg of palladium chloride and continue stirring for 30 min. Then add 20 mg of citric acid and continue stirring for 2 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0031] Example 2 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of this embodiment is as follows: (1) Dissolve 0.90 g of hydroxyacetic acid in a mixed solution (9 mL of ethanol + 51 mL of propanol) and stir for 30 min to form a uniform, stable, clear and transparent solution. Then add 0.15 g of stannous bromide and 2 mL of H2O to the mixed solution. Ultrasonicate for 10 min to produce a precipitate. Continue stirring at room temperature for 2 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0032] (2) Dissolve 60 mg of the precursor prepared in (1) in 30 mL of ethanol, stir for 20 min after ultrasonic dissolution, then add 20 mg of urea and stir for 30 min. Finally, add 4 mg of WCl6 and stir at 60 °C under nitrogen (nitrogen flow rate: 60 mL / min) for 24 h. Wash with ethanol three times and dry in an oven at 60 °C for 4 h to obtain a sample. Place the sample in a tubular furnace and heat it to 500 °C at a heating rate of 1 °C / min and keep it at this temperature for 1 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0033] (3) Dissolve 50 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 0.5 mg of palladium chloride and continue stirring for 30 min. Then add 10 mg of sodium borohydride and continue stirring for 2 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0034] Example 3 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of this embodiment is as follows: (1) Dissolve 0.28 g of oxalic acid in a mixed solution (3 mL of ethanol + 17 mL of propanol) and stir for 30 min to form a uniform, stable, clear and transparent solution. Then add 0.05 g of stannous oxalate and 1 mL of H2O to the mixed solution. Ultrasonicate for 6 min to produce a precipitate. Continue stirring at room temperature for 2 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0035] (2) Dissolve 40 mg of the precursor prepared in (1) in 20 mL of ethanol, sonicate and stir for 20 min, then add 10 mg of sodium bis(2-ethylhexyl) succinate sulfonate, stir for 20 min, and finally add 4 mg of (NH4)6H2W 12 O 40 ·xH2O, stirred at 70℃ under nitrogen (nitrogen flow rate: 50 mL / min) for 24 h, washed with ethanol three times, dried in an oven at 60℃ for 8 h to obtain a sample, placed in a tubular furnace and heated to 500℃ at a heating rate of 1℃ / min, and kept warm for 2 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0036] (3) Dissolve 100 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 1 mg of palladium nitrate and continue stirring for 30 min. Then add 10 mg of sodium borohydride and continue stirring for 2 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0037] Example 4 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of this embodiment is as follows: (1) Dissolve 0.60 g of aminosulfonic acid in a mixed solution (9 mL of ethanol + 51 mL of propanol) and stir for 30 min to form a uniform, stable, clear and transparent solution. Then add 0.10 g of stannous oxalate and 2.5 mL of H2O to the mixed solution. Ultrasonicate for 10 min to produce a precipitate. Continue stirring at room temperature for 1.5 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0038] (2) 80 mg of the precursor prepared in (1) was dissolved in 40 mL of ethanol, and the mixture was ultrasonically dissolved and stirred for 10 min. Then, 20 mg of hexadecyltrimethylammonium bromide was added and stirred for 30 min. Finally, 4 mg of K2WO4 was added and stirred at 50 °C under nitrogen (nitrogen flow rate: 60 mL / min) for 24 h. The mixture was washed with ethanol three times and dried in an oven at 60 °C for 10 h to obtain a sample. The sample was placed in a tubular furnace and heated to 500 °C at a heating rate of 2 °C / min and kept at this temperature for 2 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0039] (3) Dissolve 50 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 0.5 mg of potassium palladium oxide and continue stirring for 30 min. Then add 10 mg of ascorbic acid and continue stirring for 2 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0040] Example 5 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of this embodiment is as follows: (1) Dissolve 0.56 g of hydroxyacetic acid in a mixed solution (6 mL of ethanol + 34 mL of propanol) and stir for 20 min to form a uniform, stable, clear and transparent solution. Then add 0.08 g of stannous bromide and 2 mL of H2O to the mixed solution. Ultrasonicate for 8 min to produce a precipitate. Continue stirring at room temperature for 2 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0041] (2) Dissolve 40 mg of the precursor prepared in (1) in 20 mL of ethanol, ultrasonically dissolve and stir for 20 min, then add 10 mg of urea and stir for 30 min. Finally, add 4 mg of Na2WO4·2H2O and stir at 60°C under nitrogen (nitrogen flow rate: 50 mL / min) for 24 h. Wash with ethanol three times and dry in an oven at 60°C for 12 h to obtain a sample. Place the sample in a tubular furnace and heat it to 500°C at a heating rate of 2.5°C / min and keep it at this temperature for 1 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0042] (3) Dissolve 100 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 1 mg of palladium acetate and continue stirring for 30 min. Then add 20 mg of citric acid and continue stirring for 3 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0043] Example 6 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of this embodiment is as follows: (1) Dissolve 0.56 g of oxalic acid in a mixed solution (6 mL of ethanol + 34 mL of propanol) and stir for 30 min to form a uniform, stable, clear and transparent solution. Then add 0.08 g of stannous chloride and 2 mL of H2O to the mixed solution. Ultrasonicate for 5 min to produce a precipitate. Continue stirring at room temperature for 1 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0044] (2) Dissolve 40 mg of the precursor prepared in (1) in 20 mL of ethanol, ultrasonically dissolve and stir for 20 min, then add 10 mg of polyvinyl pyrrolidone and stir for 20 min, finally add 4 mg of WCl6 and stir at 60 °C under nitrogen (nitrogen flow rate: 40 mL / min) for 24 h. Wash with ethanol three times and dry in an oven at 60 °C for 6 h to obtain a sample. Place the sample in a tubular furnace and heat it to 500 °C at a heating rate of 5 °C / min and keep it at this temperature for 2 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0045] (3) Dissolve 100 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 1 mg of palladium chloride and continue stirring for 30 min. Then add 10 mg of sodium borohydride and continue stirring for 2 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0046] Figure 1 This is the XRD spectrum of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction obtained in this example. The product is a composite of Pd and WO3-SnO2. Figure 2 This is the SEM photo of the material. In the Pd-loaded one-dimensional WO3-SnO2 composite material, it can be clearly seen that the composite material is a porous material.

[0047] Figure 3 The response values ​​of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction to 50 ppm hydrogen at 70-130°C obtained in this embodiment. It can be seen that at 90°C, the response of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction to 50 ppm hydrogen is the highest, with a response value of 235.52, so 90°C is specified as the optimal operating temperature.

[0048] Figure 4 This is a long-term stability test of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction obtained in this embodiment within 30 days. It can be seen that the response value does not change significantly, indicating that the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction has good stability.

[0049] Example 7 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of this embodiment is as follows: (1) Dissolve 0.70 g of aminosulfonic acid in a mixed solution (6 mL of ethanol + 34 mL of propanol) and stir for 30 min to form a uniform, stable, clear and transparent solution. Then add 0.12 g of stannous oxalate and 2.2 mL of H2O to the mixed solution. Ultrasonicate for 10 min to produce a precipitate. Continue stirring at room temperature for 2 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0050] (2) Dissolve 50 mg of the precursor prepared in (1) in 25 mL of ethanol, dissolve under ultrasonication and stir for 20 min, then add 10 mg of sodium bis(2-ethylhexyl) succinate sulfonate, stir for 20 min, and finally add 4 mg of H4[Si(W3O 10)4]·xH2O, stirred at 50℃ under nitrogen (nitrogen flow rate: 60 mL / min) for 24 h, washed with ethanol three times, and dried in an oven at 60℃ for 9 h to obtain a sample, which was placed in a tubular furnace and heated to 500℃ at a heating rate of 1℃ / min and kept for 1.5 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0051] (3) Dissolve 50 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 1 mg of palladium nitrate and continue stirring for 30 min. Then add 20 mg of sodium hypophosphite and continue stirring for 2 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0052] Example 8 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction in this embodiment is as follows (1) Dissolve 0.30 g of hydroxyacetic acid in a mixed solution (3 mL of ethanol + 17 mL of propanol) and stir for 30 min to form a uniform, stable, clear and transparent solution. Then add 0.05 g of stannous oxalate and 1.5 mL of H2O to the mixed solution. Ultrasonicate for 10 min to produce a precipitate. Continue stirring at room temperature for 3 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0053] (2) Dissolve 40 mg of the precursor prepared in (1) in 20 mL of ethanol, stir for 20 min after ultrasonic dissolution, then add 10 mg of urea and stir for 20 min. Finally, add 4 mg of Na2WO4·2H2O and stir at 50 °C under nitrogen (nitrogen flow rate: 50 mL / min) for 24 h. Wash with ethanol three times and dry in an oven at 60 °C for 5 h to obtain a sample. Place the sample in a tubular furnace and heat it to 500 °C at a heating rate of 2 °C / min and keep it at this temperature for 2 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0054] (3) Dissolve 50 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 0.5 mg of potassium palladium oxide and continue stirring for 30 min. Then add 5 mg of sodium borohydride and continue stirring for 3 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0055] Example 9 The preparation method of the Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction of this embodiment is as follows: (1) Dissolve 0.50 g of oxalic acid in a mixed solution (4.5 mL of ethanol + 25.5 mL of propanol) and stir for 30 min to form a uniform, stable, clear and transparent solution. Then add 0.08 g of stannous chloride and 1.9 mL of H2O to the mixed solution. Ultrasonicate for 10 min to produce a precipitate. Continue stirring at room temperature for 2.5 h, then wash with ethanol three times and dry in an oven at 60°C to obtain the precursor.

[0056] (2) Dissolve 60 mg of the precursor prepared in (1) in 30 mL of ethanol, stir for 30 min after ultrasonic dissolution, then add 15 mg of hexadecyltrimethylammonium bromide and stir for 30 min. Finally, add 6 mg of K2WO4 and stir at 60 °C under nitrogen (nitrogen flow rate: 60 mL / min) for 24 h. Wash with ethanol three times and dry in an oven at 60 °C for 6 h to obtain a sample. Place the sample in a tubular furnace and heat it to 500 °C at a heating rate of 5 °C / min and keep it at this temperature for 2 h to obtain a one-dimensional WO3-SnO2 nanowire heterojunction.

[0057] (3) Dissolve 100 mg of one-dimensional WO3-SnO2 nanowires prepared in (2) in 20 mL of deionized water and stir for 30 min. Add 1 mg of palladium bromide and continue stirring for 30 min. Then add 20 mg of citric acid and continue stirring for 3 h. Finally, wash with deionized water and ethanol twice each. After drying in a vacuum oven at 80 °C, obtain a Pd-loaded one-dimensional WO3-SnO2 nanowire heterojunction.

[0058] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A Pd-loaded 1D WO 3 -SnO 2 Nanowire heterojunction, Features: The Pd-loaded 1D WO 3 -SnO 2 WO in nanowire heterojunction 3 and SnO 2 In the same one-dimensional nanowire structure, Pd nanoparticles are loaded on one-dimensional WO 3 -SnO 2 Nanowire heterojunction support surface.

2. The Pd-loaded one-dimensional WO according to claim 1 3 -SnO 2 Application of nanowire heterojunction as gas sensor in high sensitivity hydrogen sensor.

3. The Pd-loaded one-dimensional WO according to claim 1 3 -SnO 2 Method for preparing nanowire heterojunction, It is characterized in that The following steps are involved: (1) Preparing a precursor: adding an organic acid, a tin compound, and deionized water to an organic solvent, ultrasonically removing a precipitate, continuing to stir at room temperature, and then centrifugally washing and drying to obtain a precursor; (2) Preparation of one-dimensional WO 3 -SnO 2 Nanowire heterojunction: The precursor, organic matter and tungsten compound prepared in step (1) are dissolved in ethanol to obtain a mixed solution A, heated and stirred and reacted under nitrogen protection, centrifuged, washed and dried, and the obtained sample is calcined under high temperature conditions to obtain a one-dimensional WO 3 -SnO 2 Nanowire heterojunction; (3) Preparation of Pd-loaded one-dimensional WO 3 -SnO 2 Nanowire heterojunction: The one-dimensional WO prepared in step (2) 3 -SnO 2 The nanowire heterojunction, palladium compound and reducing agent were dissolved in deionized water, ultrasonically dissolved and stirred to obtain a mixed solution B, and centrifuged, washed and dried to obtain Pd-loaded one-dimensional WO 3 -SnO 2 Nanowire heterojunction.

4. The Pd-loaded one-dimensional WO according to claim 3 3 -SnO 2 Method for preparing nanowire heterojunction, Features: The tin compound in step (1) is one or more of stannous chloride, stannous oxalate, stannous nitrate and stannous bromide; the organic acid is one or more of oxalic acid, glycolic acid and aminosulfonic acid; and the organic solvent is at least two of ethanol, propanol, glycerol, tetrahydrofuran and n-hexane.

5. The Pd-loaded one-dimensional WO according to claim 3 3 -SnO 2 Method for preparing nanowire heterojunction, Features: In the step (1), the mass ratio of the tin compound to the organic acid is 1:5 to 1:

20.

6. The Pd-loaded one-dimensional WO according to claim 3 3 -SnO 2 Method for preparing nanowire heterojunction, Features: The tungsten compound in step (2) is Na 2 WO 4 ·2H 2 O.K 2 WO 4 NH 4 ) 6 H 2 W 12 O 40 ·xH 2 O, H 4 [Si(W 3 O 10 ) 4 ]·xH 2 O、WCl 6 The organic matter is one or more of urea, polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, and sodium bis(2-ethylhexyl) succinate sulfonate.

7. The Pd-loaded one-dimensional WO according to claim 3 3 -SnO 2 Method for preparing nanowire heterojunction, Features: The mass ratio of the precursor to the tungsten compound in step (2) is 1:0.02 to 1:0.2; the total concentration of the precursor and the tungsten compound in the mixed solution A is 1 mg / mL to 3 mg / mL, and the mass ratio of the organic matter to the precursor is 1:3 to 1:

15.

8. The Pd-loaded one-dimensional WO according to claim 3 3 -SnO 2 Method for preparing nanowire heterojunction, Features: In the step (2), the heating temperature is 50-150°C, the nitrogen flow rate is 40-100 mL / min, and the stirring reaction time is 24-48 h; the calcination temperature is 400-800°C, the heating rate is 1°C / min-5°C / min, and the calcination time is 2-3 h.

9. The Pd-loaded one-dimensional WO according to claim 3 3 -SnO 2 Method for preparing nanowire heterojunction, Features: The palladium compound in step (3) is one or more of palladium acetate, palladium chloride, potassium palladate, and palladium nitrate; the reducing agent is one or more of sodium borohydride, ascorbic acid, sodium hypophosphite, and citric acid.

10. The Pd-loaded one-dimensional WO according to claim 3 3 -SnO 2 Method for preparing nanowire heterojunction, Features: The mass ratio of the reducing agent to the palladium compound in step (3) is 1:(0.05-0.5); one-dimensional WO 3 -SnO 2 The mass ratio of nanowires to palladium compounds is 1:(0.005-0.02); one-dimensional WO in mixed solution B 3 -SnO 2 The total concentration of the nanowires and the palladium compound is 1 mg / mL to 10 mg / mL.

Citation Information

Cited By

  • Nano array for exposing SnO2 high-activity crystal face, preparation method and application of nano array in hydrogen sensing

    CN120717819A