Preparation method and application of ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial

Through the etching and calcining technology of ZIF 8 and ZIF 67 composite and polystyrene microsphere templates, cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterials were prepared, which solved the problem of poor conductivity of ZIF materials and realized hydroquinone and efficient detection of catechol, suitable for environmental monitoring.

CN119044276AInactive Publication Date: 2024-11-29ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411155012.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently detect the low concentrations of hydroquinone and catechol at the same time, and the conductivity and stability of ZIF materials are poor, which limits the detection performance of electrochemical sensors.

Method used

Cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterials (Co/Zn-HNC) were prepared by compositeing ZIF 8 with ZIF 67, using polystyrene microspheres as templates, etching and high-temperature calcination, and used to construct electrochemical sensors , improves the mass transfer rate and conductivity.

Benefits of technology

It realizes high sensitivity detection of hydroquinone and catechol, has low detection limit, and has excellent detection performance and stability in actual water samples, which is suitable for environmental monitoring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044276A_ABST
    Figure CN119044276A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial and application of the ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial in electrochemical detection of hydroquinone and catechol, and relates to the technical field of electrochemical sensing. A ZIF precursor is synthesized by taking polystyrene microspheres as a template, and cobalt and zinc loaded hollow nitrogen-doped carbon (Co / Zn-HNC) with a hollow structure is obtained after etching and high-temperature pyrolysis. The Co / Zn-HNC prepared by the method has the advantages of high conductivity, large specific surface area, good catalytic performance and the like. On the basis, the constructed Co / Zn-HNC electrochemical sensor is used for simultaneously detecting hydroquinone and catechol, has the advantages of quick response, high sensitivity, low detection limit and the like, and has good applicability in actual water sample detection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrochemical sensing technology, and in particular to a preparation method of a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial and an application thereof in electrochemical detection of hydroquinone and catechol. Background Art

[0002] Hydroquinone (HQ) and catechol (CC) are two common dihydroxybenzene isomers, which are widely used as pesticides, medicines, dyes, and photographic chemicals. However, these two isomers pose a major threat to the environment and human health due to their high toxicity and low degradability. Therefore, sensitive determination of this type of substance is of great significance for environmental monitoring. The structures and properties of these two compounds are extremely similar. Especially at low concentrations, the simultaneous detection of the two isomers of hydroquinone and catechol remains a challenge. Therefore, it is of great significance to explore sensitive detection methods for the simultaneous determination of hydroquinone and catechol.

[0003] Electrochemical sensing technology has attracted attention due to its advantages such as fast signal response, high sensitivity, low construction cost, and easy miniaturization, and has been applied to important fields such as food and drug quality control, disease marker monitoring, and environmental monitoring. The development of electrochemical sensing nanomaterials with superior performance is of great significance for further improving the detection performance of electrochemical sensors. Zeolite imidazole framework materials (ZIF) are a kind of porous crystalline nanomaterials with the characteristics of large surface area, high porosity, and rich active sites. They have been widely used in gas adsorption, catalysis, and biosensing. However, compared with metal elements and oxides, ZIF materials have weak conductivity and poor stability. In order to make full use of the structural advantages of ZIF materials and improve their performance shortcomings, they can be used as precursors to further prepare metal single atoms, nanoparticles, and oxides derived from ZIF. ZIF 8 is the most common ZIF material with zinc as the coordination center. Due to the low boiling point of zinc, it can obtain porous nitrogen-doped carbon with high specific surface area after high-temperature calcination, but its stability and conductivity are poor. In comparison, due to the higher boiling point of cobalt, ZIF 67 with cobalt as the coordination center is calcined to obtain porous nitrogen-doped carbon supported by cobalt (or cobalt compounds), which has better conductivity, stability and catalytic activity, but lower specific surface area and less nitrogen content.

[0004] In order to combine the advantages of ZIF 8 and ZIF 67, the bimetallic composite material derived from the two can not only maintain the original structural advantages, but also produce a good synergistic effect, making the mass transfer rate faster, the conductivity higher, and the catalytic active sites more. However, there is no related report in the prior art. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the present invention provides a preparation method and application of ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterials. The present invention uniformly combines two ZIF materials on polystyrene microspheres, and obtains ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon (Co / Zn-HNC) by etching and high-temperature calcination. The material is further used to construct a new electrochemical sensor, which exhibits excellent detection sensing performance for hydroquinone and catechol, with high sensitivity and low detection limit. The sensor has been successfully used to simultaneously detect the content of hydroquinone and catechol in tap water.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterials comprises the following steps:

[0008] (1) Preparation of polystyrene microspheres

[0009] Add an aqueous solution containing styrene, methyl methacrylate, acrylic acid and ammonium bicarbonate into a 250ml three-necked flask, stir and heat to a certain temperature, then add ammonium persulfate to the mixed solution, continue to heat to a certain temperature to continue the reaction, collect the product by centrifugation, and wash with water. The synthesized sample is freeze-dried and ground to obtain a white powder, which is the prepared polystyrene microspheres;

[0010] (2) Preparation of Co / Zn-HNC precursor

[0011] The polystyrene microspheres obtained in step (1) are added to methanol, and after ultrasonication, polyvinyl pyrrolidone is added and stirred to form a dispersion A; a certain amount and a certain proportion of zinc nitrate hexahydrate and cobalt nitrate hexahydrate are dissolved in methanol to form a solution B; the solution B is quickly added to the dispersion A, and the mixture is stirred and mixed evenly; dimethyl imidazole is dissolved in a methanol solution to obtain a solution C, and the solution C is added dropwise to the mixture of dispersions A and B, and the stirring is continued until the reaction is completed, the product is collected by centrifugation, washed with methanol, and the synthesized sample is vacuum dried to obtain a purple powder, which is a precursor;

[0012] (3) Etching and pyrolysis

[0013] The precursor synthesized in step (2) is immersed in N,N-dimethylformamide and stirred at room temperature to remove the core of the polystyrene microspheres. The product is collected by centrifugation, washed with methanol, and the synthesized sample is vacuum dried; the synthesized sample is heated to a desired temperature at a certain heating rate under N2 atmosphere, then maintained for a certain time, and cooled to room temperature to obtain the product Co / Zn-HNC.

[0014] Furthermore, the diameter of the polystyrene microspheres in step (1) is 100-200 nm.

[0015] Furthermore, in step (1), the ratio of the aqueous solutions of styrene, methyl methacrylate, acrylic acid, ammonium bicarbonate and ammonium persulfate is: 19 ml: 1 ml: 0.84 ml: 0.45 g: 0.48 g.

[0016] Furthermore, in step (1), the first heating temperature is 70° C., the second heating temperature is 80° C., and the reaction time is 12 h.

[0017] Furthermore, in step (2), the mass ratio of polystyrene microspheres, zinc nitrate hexahydrate, cobalt nitrate hexahydrate, and dimethylimidazole is 1:1.59:0.39:5.33.

[0018] Furthermore, in step (2), the ultrasonic dispersion time of the polystyrene microspheres is 30 min, and the stirring time is 2.5 h; the stirring time for uniformly mixing the dispersion A and the solution B is 30 min, and the stirring time after adding the solution C is 1 h.

[0019] Furthermore, in step (3), the ratio of the precursor to N,N-dimethylformamide is 100 mg:50 ml, the etching temperature is room temperature, and the etching time is 24 h.

[0020] Furthermore, in step (3), the heating rate used for pyrolysis is 5°C / min, the pyrolysis temperature is 800°C, and the pyrolysis time is 3h.

[0021] Another object of the present invention is to provide an application of the nanomaterial prepared by the above preparation method in electrochemical detection of hydroquinone and catechol.

[0022] Specifically, the nanomaterial can be used to construct an electrochemical sensor and be used to simultaneously and sensitively detect two isomers of hydroquinone and catechol in water.

[0023] Beneficial effects of the present invention:

[0024] The object of the present invention is to provide a method for preparing hollow nitrogen-doped carbon derived from cobalt and zinc. Compared with traditional ZIF materials, this method uses polystyrene microspheres as templates. After etching, the polystyrene microspheres are dissolved to obtain a hollow structure, so that the active area of ​​the prepared catalyst is increased and the mass transfer and charge transfer capacity is enhanced. Cobalt and zinc composite ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon materials have a good synergistic effect, which makes the mass transfer and charge transfer rate faster, the conductivity higher, and the catalytic active sites more. The catalyst is used as an electrode material to construct a new electrochemical sensor, which shows excellent and stable performance in the electrochemical detection of hydroquinone and catechol test conditions. The constructed electrochemical sensor has the advantages of low cost, rapid response, convenience and speed, and can be actually applied to the simultaneous detection of low-concentration hydroquinone and catechol in actual water samples, and has practical application value in environmental analysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described below in conjunction with the accompanying drawings.

[0026] Figure 1 This is a TEM electron microscope image of the cobalt and zinc loaded hollow nitrogen-doped carbon (Co / Zn-HNC) prepared in Example 1.

[0027] Figure 2 It is a comparison chart of X-ray diffraction (XRD) of five different catalysts in Example 1, Example 2, Example 3, Example 4, and Example 5 and a single substance Co standard card.

[0028] Figure 3 The electrochemical performance response comparison diagram of five different catalysts for hydroquinone and catechol in Example 1, Example 2, Example 3, Example 4 and Example 5 ( Figure 3 a is the bar graph of electrochemical response of different catalysts to two catalysts. Figure 3 b, 3c are DPV curves of electrochemical responses of different catalysts to hydroquinone and catechol respectively);

[0029] Figure 4 The performance of the catalyst Co / Zn-HNC in Example 1 on hydroquinone and catechol under different pH conditions was tested and pH optimization was performed ( Figure 4 a is the electrochemical response bar graph of the catalyst to two substances under different pH conditions. Figure 4 b, 4c are DPV curves of electrochemical response of hydroquinone and catechol under different pH conditions respectively);

[0030] Figure 5 The selectivity test of the catalyst Co / Zn-HNC in Example 1 for simultaneous detection of hydroquinone and catechol;

[0031] Figure 6The stability test of hydroquinone was performed on the catalyst Co / Zn-HNC of Example 1;

[0032] Figure 7 The detection limit test of the catalyst Co / Zn-HNC in Example 1 for simultaneous detection of hydroquinone and catechol ( Figure 7 a is the DPV curve of electrochemical response of hydroquinone and catechol at different concentrations. Figure 7 b, 7c are the current-concentration fitting curves of hydroquinone and catechol at different concentrations, respectively;

[0033] Figure 8 This is a test diagram of the catalyst Co / Zn-HNC in Example 1 for simultaneous detection of hydroquinone and catechol in actual samples. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] Step 1: Add 300 mg of polystyrene microspheres to 60 ml of methanol, ultrasonicate for 30 min, add 1 g of polyvinyl pyrrolidone, stir for 2.5 h to form dispersion A; dissolve 476 mg of Zn(NO3)2·6H2O and 116 mg of Co(NO3)2·6H2O in 5 ml of methanol to form solution B; quickly add solution B to solution A, stir for 30 min, mix well, weigh 1.66 g of dimethylimidazole and dissolve it in 15 ml of methanol solution, add the solution dropwise to dispersion A, and continue to react for 1 h. Collect the product by centrifugation and wash it with methanol 3 times. The synthesized sample was vacuum dried.

[0037] Step 2: Weigh 100 mg of the precursor synthesized in the first step and soak it in 50 ml of N,N-dimethylformamide. Continue stirring at room temperature for 24 hours to remove the core of the polystyrene microspheres. Collect the product by centrifugation and wash it with methanol three times. The synthesized sample is vacuum dried.

[0038] Step 3: The sample synthesized in the second step was heated to 800°C at a heating rate of 5°C / min under N2 atmosphere, kept for 3 hours and then cooled to room temperature to obtain cobalt and zinc loaded hollow nitrogen-doped carbon (Co / Zn-HNC). Its morphology is as follows Figure 1 shown.

[0039] Example 2

[0040] Step 1: Add 300 mg of polystyrene microspheres to 60 ml of methanol, ultrasonicate for 30 min, add 1 g of polyvinyl pyrrolidone, stir for 2.5 h to form dispersion A; dissolve 600 mg of Zn(NO3)2·6H2O in 5 ml of methanol to form solution B; quickly add solution B to solution A, stir for 30 min, and after mixing evenly, weigh 1.66 g of dimethylimidazole and dissolve it in 15 ml of methanol solution, add the solution dropwise to dispersion A, and continue the reaction for 1 h. Collect the product by centrifugation and wash it with methanol 3 times. The synthesized sample was vacuum dried.

[0041] Step 2: Weigh 100 mg of the intermediate synthesized in the first step and soak it in 50 ml of N,N-dimethylformamide. Continue stirring at room temperature for 24 hours to remove the core of the polystyrene microspheres. Collect the product by centrifugation and wash it with methanol three times. The synthesized sample is vacuum dried.

[0042] Step 3: The sample synthesized in the second step was heated to 800°C in a N2 atmosphere at a heating rate of 5°C / min, maintained for 3 h, and then cooled to room temperature to obtain zinc-loaded hollow nitrogen-doped carbon (Zn-HNC).

[0043] Example 3

[0044] Step 1: Weigh 600 mg Zn(NO3)2·6H2O and dissolve it in 65 ml methanol to form solution A; weigh 1.66 g dimethylimidazole and dissolve it in 15 ml methanol to form solution B. Add solution B dropwise to dispersion A and continue the reaction for 1 hour. Collect the product by centrifugation and wash it with methanol three times. The synthesized sample is vacuum dried.

[0045] Step 2: Heat the sample synthesized in the first step to 800°C in a N2 atmosphere at a heating rate of 5°C / min, keep it for 3 hours and then cool it to room temperature to obtain zinc-loaded solid nitrogen-doped carbon (Zn-NC).

[0046] Example 4

[0047] Step 1: Weigh 600 mg Co(NO3)2·6H2O and dissolve it in 65 ml methanol to form solution A; weigh 1.66 g dimethylimidazole and dissolve it in 15 ml methanol to form solution B. Add solution B dropwise to dispersion A and continue the reaction for 1 hour. Collect the product by centrifugation and wash it with methanol three times. The synthesized sample is vacuum dried.

[0048] Step 2: Heat the sample synthesized in the first step to 800°C in a N2 atmosphere at a heating rate of 5°C / min, keep it for 3 hours and then cool it to room temperature to obtain cobalt-loaded solid nitrogen-doped carbon (Co-NC).

[0049] Example 5

[0050] Step 1: Weigh 476 mg Zn(NO3)2·6H2O and 116 mg Co(NO3)2·6H2O and dissolve them in 65 ml methanol to form solution A; weigh 1.66 g dimethylimidazole and dissolve it in 15 ml methanol to form solution B. Add solution B dropwise to dispersion A and continue the reaction for 1 hour. Collect the product by centrifugation and wash it with methanol three times. The synthesized sample is vacuum dried.

[0051] Step 2: Heat the sample synthesized in the first step to 800°C in a N2 atmosphere at a heating rate of 5°C / min, keep it for 3 hours and then cool it to room temperature to obtain cobalt and zinc loaded solid nitrogen-doped carbon (Co / Zn-NC).

[0052] The X-ray diffraction (XRD) comparison diagrams of five different catalysts and a single substance Co standard card in Example 1, Example 2, Example 3, Example 4, and Example 5 are shown in FIG. Figure 2 As shown; it can be seen that compared with the diffraction peaks of Zn-HNC and Co-NC, Co / Zn-HNC has obvious diffraction peaks of Co element, indicating that the material was successfully prepared.

[0053] Application Example 1

[0054] (1) Pretreatment of working electrode

[0055] The working electrode used was a glassy carbon electrode (GCE, 3 mm in diameter), which was carefully polished on the suede surface with micron-grade Al2O3 powder. Each polishing time was 3 min. The polished glassy carbon electrode was rinsed with deionized water to remove the polishing powder on the surface, then ultrasonically cleaned with deionized water, and finally dried under an infrared lamp.

[0056] (2) Modified glassy carbon electrode

[0057] 2.5 mg of the five catalysts prepared in Example 1, Example 2, Example 3, Example 4, and Example 5, namely Co / Zn-HNC, Zn-HNC, Zn-NC, Co-NC, and Co / Zn-NC, were weighed and dispersed in 25 μL of Nafion (5wt%), 250 μL of deionized water, and 225 μL of anhydrous ethanol mixed solution, and then uniformly dispersed by ultrasonication to obtain dispersants of five different catalysts. 5 μL of the catalyst dispersion was dropped on a polished glassy carbon electrode and dried under an infrared lamp to obtain a catalyst-modified electrode.

[0058] (3) Electrochemical test

[0059] Electrochemical tests were performed on the electrodes modified with five catalysts to compare their electrochemical responses to hydroquinone and catechol. The electrochemical test was performed using a CHI1040C multi-channel potentiostat, in which the catalyst-modified glassy carbon electrode was the working electrode, the platinum wire electrode was the counter electrode, and the Ag / AgCl electrode was the reference electrode. 0.1M PBS solution was used as the electrolyte for the electrochemical performance test, and the electrochemical test method was differential pulse voltammetry (DPV).

[0060] The DPV performance test results of different catalysts in this application example are as follows: Figure 3 The DPV curve and bar graph are shown in the figure. Comparing the electrochemical performance of Co / NC and Zn / NC synthesized by ZIF67 and ZIF8 to the two catalysts, it can be seen that Co has a better electrochemical response than Zn. Therefore, we composited the two metals to obtain Co / Zn-NC, which has improved performance compared to Zn / NC and Zn / HNC. On this basis, we introduced polystyrene microspheres as templates, adsorbed the ZIF materials of the two metals on the polystyrene microspheres at the same time, and obtained Co / Zn-HNC catalyst after etching and high-temperature calcination. This catalyst has a very high electrochemical response to the two substances.

[0061] Application Example 2

[0062] (1) Pretreatment of working electrode

[0063] The working electrode used was a glassy carbon electrode (GCE, 3 mm in diameter), which was carefully polished on the suede surface with micron-grade Al2O3 powder. Each polishing time was 3 min. The polished glassy carbon electrode was rinsed with deionized water to remove the polishing powder on the surface, then ultrasonically cleaned with deionized water, and finally dried under an infrared lamp.

[0064] (2) Modified glassy carbon electrode

[0065] 2.5 mg of the Co / Zn-HNC catalyst prepared in Example 1 was weighed and dispersed in a mixed solution of 25 μL of Nafion (5 wt%), 250 μL of deionized water, and 225 μL of anhydrous ethanol, and then uniformly dispersed by ultrasonication to obtain a dispersant. 5 μL of the catalyst dispersion was dropped onto a polished glassy carbon electrode and dried under an infrared lamp to obtain a catalyst-modified electrode.

[0066] (3) Electrochemical test

[0067] Electrochemical tests were performed on the electrodes modified with Co / Zn-HNC catalysts, pH was optimized, and the performance of the catalyst under different pH conditions was compared. The electrochemical tests were performed using a CHI1040C multi-channel potentiostat, in which the catalyst-modified glassy carbon electrode was the working electrode, the platinum wire electrode was the counter electrode, and the Ag / AgCl electrode was the reference electrode. 0.1M PBS solution was used as the electrolyte for electrochemical performance tests, and the electrochemical test method was differential pulse voltammetry (DPV).

[0068] The performance test results of Co / Zn-HNC catalyst in this application example are as follows Figure 4 The test results compare the performance of the catalyst under different pH conditions. By comparing the DPV curve and the bar chart, it can be seen that when the pH value is 7.0, the catalyst responds best.

[0069] Application Example 3

[0070] (1) Pretreatment of working electrode

[0071] The working electrode used was a glassy carbon electrode (GCE, 3 mm in diameter), which was carefully polished on the suede surface with micron-grade Al2O3 powder. Each polishing time was 3 min. The polished glassy carbon electrode was rinsed with deionized water to remove the polishing powder on the surface, then ultrasonically cleaned with deionized water, and finally dried under an infrared lamp.

[0072] (2) Modified glassy carbon electrode

[0073] 2.5 mg of the Co / Zn-HNC catalyst prepared in Example 1 was weighed and dispersed in a mixed solution of 25 μL of Nafion (5 wt%), 250 μL of deionized water, and 225 μL of anhydrous ethanol, and then uniformly dispersed by ultrasonication to obtain a dispersant. 5 μL of the catalyst dispersion was dropped onto a polished glassy carbon electrode and dried under an infrared lamp to obtain a catalyst-modified electrode.

[0074] (3) Electrochemical test

[0075] Electrochemical tests were performed on the electrodes modified with Co / Zn-HNC catalysts to test the selectivity of the catalyst. The electrochemical test was performed using a CHI1040C multi-channel potentiostat, in which the catalyst-modified glassy carbon electrode was the working electrode, the platinum wire electrode was the counter electrode, and the Ag / AgCl electrode was the reference electrode. 0.1M PBS solution was used as the electrolyte for the electrochemical performance test, and the electrochemical test method was differential pulse voltammetry (DPV).

[0076] The selectivity test results of the catalyst in this application example are as follows: Figure 5The test results compared the addition of 20 μM hydroquinone and catechol and 200 μM interferents, including resorcinol (RS), glucose (Glu), bisphenol S (BPS), ascorbic acid (ASA), urea (Urea), Ca + , Cu 2+ Mg 2+ 、Na + The electrochemical response of the catalyst showed that the catalyst still exhibited good selectivity for hydroquinone and catechol in the presence of relatively high concentrations of interferents.

[0077] Application Example 4

[0078] (1) Pretreatment of working electrode

[0079] The working electrode used was a glassy carbon electrode (GCE, 3 mm in diameter), which was carefully polished on the suede surface with micron-grade Al2O3 powder. Each polishing time was 3 min. The polished glassy carbon electrode was rinsed with deionized water to remove the polishing powder on the surface, then ultrasonically cleaned with deionized water, and finally dried under an infrared lamp.

[0080] (2) Modified glassy carbon electrode

[0081] 2.5 mg of the Co / Zn-HNC catalyst prepared in Example 1 was weighed and dispersed in a mixed solution of 25 μL of Nafion (5 wt%), 250 μL of deionized water, and 225 μL of anhydrous ethanol, and then uniformly dispersed by ultrasonication to obtain a dispersant. 5 μL of the catalyst dispersion was dropped onto a polished glassy carbon electrode and dried under an infrared lamp to obtain a catalyst-modified electrode.

[0082] (3) Electrochemical test

[0083] Electrochemical tests were performed on the electrodes modified with Co / Zn-HNC catalysts to test the stability of the catalyst. The electrochemical test was performed using a CHI1040C multi-channel potentiostat, in which the catalyst-modified glassy carbon electrode was the working electrode, the platinum wire electrode was the counter electrode, and the Ag / AgCl electrode was the reference electrode. 0.1M PBS solution was used as the electrolyte for the electrochemical performance test, and the electrochemical test method was differential pulse voltammetry (DPV).

[0084] The stability test results of the catalyst in this application example are as follows: Figure 6 The test results show that the catalyst still maintains a stable electrochemical response and a good standard deviation value (RSD, 2.06%) after 20 consecutive tests, which shows that the electrochemical sensor has excellent stability.

[0085] Application Example 5

[0086] (1) Pretreatment of working electrode

[0087] The working electrode used was a glassy carbon electrode (GCE, 3 mm in diameter), which was carefully polished on the suede surface with micron-grade Al2O3 powder. Each polishing time was 3 min. The polished glassy carbon electrode was rinsed with deionized water to remove the polishing powder on the surface, then ultrasonically cleaned with deionized water, and finally dried under an infrared lamp.

[0088] (2) Modified glassy carbon electrode

[0089] 2.5 mg of the Co / Zn-HNC catalyst prepared in the example was weighed and dispersed in a mixed solution of 25 μL of Nafion (5 wt%), 250 μL of deionized water, and 225 μL of anhydrous ethanol, and then uniformly dispersed by ultrasonication to obtain a dispersant. 5 μL of the catalyst dispersion was dropped onto a polished glassy carbon electrode and dried under an infrared lamp to obtain a catalyst-modified electrode.

[0090] (3) Electrochemical test

[0091] The electrode modified with Co / Zn-HNC catalyst was electrochemically tested to test the detection limit and linear range of the catalyst for simultaneous detection of hydroquinone and catechol. The electrochemical test was performed using a CHI1040C multi-channel constant potential instrument, in which the catalyst-modified glassy carbon electrode was the working electrode, the platinum wire electrode was the counter electrode, and the Ag / AgCl electrode was the reference electrode. 0.1M PBS solution was used as the electrolyte for the electrochemical performance test, and the electrochemical test method was differential pulse voltammetry (DPV).

[0092] The detection limit and linear range test results of the catalyst for simultaneous detection of hydroquinone and catechol in this application example are as follows: Figure 7 As shown, the test results show that the catalyst has excellent electrochemical response for the simultaneous detection of hydroquinone and catechol in the linear ranges of 1μM-20μM and 20μM-100μM, and the detection limits of hydroquinone and catechol are 0.002μM and 0.003μM, respectively.

[0093] Application Example 6

[0094] (1) Pretreatment of working electrode

[0095] The working electrode used was a glassy carbon electrode (GCE, 3 mm in diameter), which was carefully polished on the suede surface with micron-grade Al2O3 powder. Each polishing time was 3 min. The polished glassy carbon electrode was rinsed with deionized water to remove the polishing powder on the surface, then ultrasonically cleaned with deionized water, and finally dried under an infrared lamp.

[0096] (2) Modified glassy carbon electrode

[0097] 2.5 mg of the Co / Zn-HNC catalyst prepared in Example 1 was weighed and dispersed in a mixed solution of 25 μL of Nafion (5 wt%), 250 μL of deionized water, and 225 μL of anhydrous ethanol, and then uniformly dispersed by ultrasonication to obtain a dispersant. 5 μL of the catalyst dispersion was dropped onto a polished glassy carbon electrode and dried under an infrared lamp to obtain a catalyst-modified electrode.

[0098] (3) Electrochemical test

[0099] Electrochemical tests were performed on the electrodes modified with Co / Zn-HNC catalysts to test the performance of the catalysts for actual sample detection. The electrochemical test was performed using a CHI1040C multi-channel potentiostat, in which the catalyst-modified glassy carbon electrode was the working electrode, the platinum wire electrode was the counter electrode, and the Ag / AgCl electrode was the reference electrode. 0.1M PBS and laboratory tap water solutions were used as electrolytes for electrochemical performance tests, and the electrochemical test method was differential pulse voltammetry (DPV).

[0100] The actual sample test results of the catalyst in this application example are as follows Figure 8 The test results show that when 2 μM hydroquinone and catechol were added to PBS and tap water solutions for electrochemical detection, the recovery rate of hydroquinone and catechol in the actual tap water sample was about 99.4% and 97.9% respectively in the low concentration of the catalyst compared with the PBS solution, which proves that the constructed electrochemical sensor can realize the important application of detecting low concentrations of hydroquinone and catechol in actual water samples.

[0101] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.

Claims

1. A method for preparing ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterials, characterized in that: The following steps are involved: (1) Preparation of polystyrene microspheres An aqueous solution containing styrene, methyl methacrylate, acrylic acid and ammonium bicarbonate is added to a three-necked flask, stirred and heated to a certain temperature, and then ammonium persulfate is added to the mixed solution, and the temperature is continued to be raised to a certain temperature to continue the reaction, and the product is collected by centrifugation, washed with water, and freeze-dried and ground to obtain a white powder, which is polystyrene microspheres; (2) Preparation of Co / Zn-HNC precursor The polystyrene microspheres obtained in step (1) are added to methanol, and after ultrasonication, polyvinyl pyrrolidone is added and stirred to form a dispersion A; a certain amount and a certain proportion of zinc nitrate hexahydrate and cobalt nitrate hexahydrate are dissolved in methanol to form a solution B; the solution B is quickly added to the dispersion A, and the mixture is stirred and mixed evenly; dimethyl imidazole is dissolved in a methanol solution to obtain a solution C, and the solution C is added dropwise to the mixture of the dispersions A and B, and the stirring is continued until the reaction is completed, the product is collected by centrifugation, washed with methanol, and vacuum dried to obtain a purple powder, which is a Co / Zn-HNC precursor; (3) Etching and pyrolysis The precursor synthesized in step (2) is immersed in N,N-dimethylformamide and stirred continuously at room temperature to remove the inner core of the polystyrene microspheres. The product is collected by centrifugation, washed with methanol, and then vacuum dried. The product is heated to the desired temperature at a certain heating rate under a N2 atmosphere, and then maintained for a certain period of time and cooled to room temperature to obtain the product.

2. The method for preparing a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial according to claim 1, characterized in that: The diameter of the polystyrene microspheres in step (1) is 100-200 nm.

3. The method for preparing a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial according to claim 1, characterized in that: In step (1), the dosage ratio of the aqueous solution of styrene, methyl methacrylate, acrylic acid, ammonium bicarbonate and ammonium persulfate is 19 ml: 1 ml: 0.84 ml: 0.45 g: 0.48 g.

4. The method for preparing a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial according to claim 1, characterized in that: The first heating temperature in step (1) is 70°C, the second heating temperature is 80°C, and the reaction time is 12h.

5. The method for preparing a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial according to claim 1, characterized in that: In step (2), the mass ratio of polystyrene microspheres, zinc nitrate hexahydrate, cobalt nitrate hexahydrate, and dimethylimidazole is 1:1.59:0.39:5.

33.

6. The method for preparing a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial according to claim 1, characterized in that: In step (2), the ultrasonic dispersion time of the polystyrene microspheres is 30 min, and the stirring time is 2.5 h; the stirring time for uniformly mixing the dispersion A and the solution B is 30 min, and the stirring time after adding the solution C is 1 h.

7. The method for preparing a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial according to claim 1, characterized in that: In step (3), the ratio of precursor to N,N-dimethylformamide is 100 mg:50 ml, the etching temperature is room temperature, and the etching time is 24 h.

8. The method for preparing a ZIF-derived cobalt and zinc-loaded hollow nitrogen-doped carbon nanomaterial according to claim 1, characterized in that: The heating rate used for pyrolysis in step (3) is 5°C / min, the pyrolysis temperature is 800°C, and the pyrolysis time is 3h.

9. Application of the nanomaterial prepared by the preparation method according to any one of claims 1 to 8 in electrochemical detection of hydroquinone and catechol.

10. The use according to claim 9, characterized in that: The nanomaterial can be used to construct an electrochemical sensor and is used to simultaneously and sensitively detect two isomers of hydroquinone and catechol in water.

Citation Information

Patent Citations

  • Preparation method for ammonium polyphosphate / polystyrene core-shell microspheres

    CN102850592A

  • Modified electrode for detecting pyrocatechol and hydroquinone and preparation method thereof

    CN103901087A

  • Preparation method of 2-methylimidazole and zinc complex with hierarchical porous structure

    CN105837509A

  • Catalyst for preparation of 2,3,5-trimethylhydroquinone by hydrogenation of 2,3,5-trimethylbenzoquinone and preparation method of catalyst

    CN110339851A

  • Preparation method of 3D-ZIF8@zif67 for lithium-sulfur battery cathode material

    CN110611099A