Treatment method of electroplating liquid and testing method of dispersing agent in sample to be tested

By adding an acid neutralizing liquid to the graphene plating solution, the sodium stannate is converted to stannate acid and removed by filtration, the problem of sodium stannate precipitation in an acidic environment is solved, ensuring the accuracy and equipment of liquid chromatography testing The safety of the coating improves the uniformity of the coating and the reliability of the testing.

CN119044365APending Publication Date: 2024-11-29WENZHOU TAIYU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411312166.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In graphene electroplating solution, the crystallization of sodium stannate under acidic environment leads to clogging of the test equipment, affecting the accuracy of liquid chromatography test and equipment safety.

Method used

By adding the alkali in the acid neutralizing liquid neutralizes the electroplating solution, converting sodium stannate to stannate acid, filtration and removing it, preventing it from reacting with the acidic mobile phase to form precipitation. Microporous filter membrane filtration and liquid chromatography test are used to ensure the test The system is operating normally.

Benefits of technology

It effectively avoids the problem of precipitation blockage of sodium stannate, improves the protection of the test system and the accuracy of subsequent tests, and ensures the uniform dispersion of the plating solution and the quality of the plating layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044365A_ABST
    Figure CN119044365A_ABST
Patent Text Reader

Abstract

The invention discloses an electroplating liquid treatment method and a method for testing a dispersing agent in a to-be-tested sample, and relates to the technical field of analysis and testing. The treatment method of the electroplating solution comprises the following steps: providing an acidic neutralization solution and an electroplating solution, wherein the electroplating solution comprises sodium stannate, a dispersing agent and graphene; and mixing the acidic neutralization solution and the electroplating solution, carrying out first filtration, and removing the precipitate to obtain a sample to be detected. According to the treatment method of the electroplating solution, the acid neutralization solution is added into the electroplating solution, the acid neutralization solution can neutralize excessive alkali in the electroplating solution, hydrogen ions in the acid neutralization solution can be combined with sodium stannate to enable the sodium stannate to be converted into stannic acid to be separated out, the stannic acid is removed through filtering, and the electroplating solution is obtained. The method can prevent sodium stannate from reacting with an acidic mobile phase of liquid chromatography to generate precipitates which block a test system and affect liquid chromatography test, and improves the protection of the test system and the accuracy of subsequent test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of testing and analysis, and in particular to a method for processing an electroplating solution and a method for testing a dispersant in a sample to be tested. Background Art

[0002] Graphene is a sp 2 Two-dimensional nanomaterials with hybrid-connected single carbon atomic layers have excellent properties such as high conductivity, high thermal conductivity, high strength, high flexibility, strong chemical inertness, and excellent gas barrier properties. They show great application potential in electrical conductivity, thermal conductivity, anti-static, anti-corrosion coatings, and metal current collector materials.

[0003] Due to the strong π-π bond between graphene sheet particles, agglomeration easily occurs, resulting in poor uniform dispersion of graphene in the solution system, which seriously affects the application of graphene in coatings and plating. In order to improve the uniform dispersion of graphene in liquid phase solutions, a dispersant is usually introduced to disperse the graphene particles so that they can be evenly dispersed to achieve the smooth progress of the electrodeposition process. The dispersant molecules ionize the hydrophilic end and the graphene-philic end in the aqueous solution, and the graphene-philic end is connected to the graphene particles and then coated on the periphery of the graphene particles. Due to the electrostatic repulsion of the dispersant molecules, the graphene particles are dispersed.

[0004] In the copper-tin alloy graphene electroplating solution, sodium stannate is usually used as the main salt of the tin plating layer. The optimized plating solution system is usually a neutral solution. When the pH becomes smaller, that is, when the system becomes acidic, it will affect the solubility of the main salt sodium stannate, causing its crystallization. The test method for the dispersant in the graphene electroplating solution system usually uses liquid chromatography testing, and the fluidity is an acidic solution. When the injection test is performed, the test solution contacts the mobile phase, which will cause the main salt sodium stannate to precipitate, block the liquid chromatography test system, affect subsequent tests, and even cause damage to the test equipment. Summary of the invention

[0005] In view of this, the present application provides a method for treating an electroplating solution and a method for testing a dispersant in a sample to be tested.

[0006] The embodiment of the present application is implemented as follows. In a first aspect, the embodiment of the present application provides a method for treating an electroplating solution, comprising the following steps:

[0007] Providing an acidic neutralizing solution and an electroplating solution, wherein the electroplating solution comprises sodium stannate, a dispersant and graphene;

[0008] The acidic neutralization solution and the electroplating solution are mixed, and the precipitate is removed after a first filtration to obtain a sample to be tested.

[0009] Optionally, in some embodiments of the present application, the acidic neutralization solution comprises an acid and a first diluent; and / or

[0010] The dispersant includes one or more of sulfonates, sulfates, and polyethers; and / or

[0011] The volume ratio of the acidic neutralization solution to the electroplating solution is (60-80):10; and / or

[0012] The sample to be tested includes the dispersant.

[0013] Optionally, in some embodiments of the present application, the acid includes one or more of phosphoric acid, formic acid, and acetic acid; and / or

[0014] The first diluent comprises water; and / or

[0015] The sulfonates include one or more of sodium polynaphthalene sulfonate and sodium dodecylbenzene sulfonate; and / or

[0016] The sulfates include sodium lauryl sulfate; and / or

[0017] The polyethers include alkylphenol polyoxyethylene ethers; and / or

[0018] In the acidic neutralization solution, the volume ratio of the acid to the diluent is (51-59):(21-29).

[0019] Optionally, in some embodiments of the present application, in the electroplating solution, the mass concentration of the graphene is 0.5 g / L to 1.5 g / L; and / or

[0020] In the electroplating solution, the mass concentration of the sodium stannate is 100 g / L to 145 g / L; and / or

[0021] The electroplating solution also includes one or more of a solvent, a metal salt, and an alkali.

[0022] Optionally, in some embodiments of the present application, the solvent is selected from one or more of water, ethanol, isopropanol, N-methylpyrrolidone, dichloromethane, xylene, dichlorobenzene, ethylene glycol, and toluene; and / or

[0023] The metal salt comprises a copper salt, and the copper salt comprises one or more of cuprous cyanide, copper sulfate, copper chloride, and copper pyrophosphate; and / or

[0024] In the electroplating solution, the mass concentration of the copper salt is 5 g / L to 20 g / L; and / or

[0025] The alkali comprises one or more of potassium hydroxide and sodium hydroxide; and / or

[0026] In the electroplating solution, the mass concentration of the alkali is 5 g / L to 15 g / L.

[0027] Optionally, in some embodiments of the present application, the mixing of the acidic neutralization solution and the electroplating solution further comprises: adding a second diluent to obtain a mixed solution, and performing the first filtration on the mixed solution; wherein,

[0028] The second diluent comprises water; and / or

[0029] The volume ratio of the electroplating solution to the mixed solution is 10:(100-500); and / or

[0030] The method of adding the second diluent includes fixing the volume.

[0031] Optionally, in some embodiments of the present application, after mixing the acidic neutralization solution and the electroplating solution, stirring is further included, and the stirring time is 20 minutes to 50 minutes; and / or

[0032] The first filtering method includes microporous membrane filtration.

[0033] In a second aspect, the present application also provides a method for testing a dispersant in a sample to be tested, comprising the following steps:

[0034] Providing a sample to be tested after being treated by any of the above-mentioned electroplating solution treatment methods;

[0035] The sample to be tested is subjected to a liquid chromatography test to obtain the concentration of the dispersant.

[0036] Optionally, in some embodiments of the present application, the liquid chromatography test on the sample to be tested includes: after the sample to be tested is subjected to a second filtration, adding the sample to a chromatographic bottle for liquid chromatography test; wherein the second filtration method is needle filter filtration; and / or

[0037] The concentration of the dispersant is the volume concentration of the dispersant.

[0038] Optionally, in some embodiments of the present application, the mobile phase of the liquid chromatography test comprises a mixture of methanol and an aqueous phosphoric acid solution; wherein the volume ratio of the methanol to the aqueous phosphoric acid solution is (25-60): (40-75); and / or

[0039] The flow rate of the mobile phase of the liquid chromatography test is 0.8 mL / min to 1.5 mL / min; and / or

[0040] The wavelength of the ultraviolet detector of the liquid chromatography test is 300nm to 345nm; and / or

[0041] The temperature of the column oven of the liquid chromatography test is 28°C to 35°C; and / or

[0042] The elution time of the liquid chromatography test is 18 min to 45 min.

[0043] The present application provides a method for treating an electroplating solution, wherein an acidic neutralizing solution is added to the electroplating solution. The acidic neutralizing solution can neutralize excess alkali in the electroplating solution. The hydrogen ions in the acidic neutralizing solution can also combine with sodium stannate to convert it into stannic acid for precipitation. The stannic acid is removed by filtering, thereby preventing the sodium stannate from reacting with the acidic mobile phase of the liquid chromatography to generate a precipitate that blocks the test system and affects the liquid chromatography test, thereby improving the protection of the test system and the accuracy of subsequent tests. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0045] Figure 1 is a flow chart of a method for treating an electroplating solution provided in an embodiment of the present application;

[0046] Figure 2 It is a flow chart of a method for testing a dispersant in a sample to be tested provided in an embodiment of the present application. DETAILED DESCRIPTION

[0047] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0048] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0049] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0050] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or several", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0051] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0052] The technical solution of this application is as follows:

[0053] First, see Figure 1 The present invention provides a method for treating an electroplating solution, comprising the following steps:

[0054] S11, providing an acidic neutralization solution and an electroplating solution, wherein the electroplating solution comprises sodium stannate, a dispersant and graphene;

[0055] S12, mixing the acidic neutralization solution and the electroplating solution, performing a first filtration to remove the precipitate, and obtaining a sample to be tested.

[0056] It can be understood that the electroplating solution contains sodium stannate and graphene, and the electroplating solution can be a copper-tin alloy graphene electroplating solution.

[0057] The present application provides a method for treating an electroplating solution, wherein an acidic neutralizing solution is added to the electroplating solution. The acidic neutralizing solution can neutralize excess alkali in the electroplating solution. The hydrogen ions in the acidic neutralizing solution can also combine with sodium stannate to convert it into stannic acid for precipitation. The stannic acid is removed by filtering, thereby preventing the sodium stannate from reacting with the acidic mobile phase of the liquid chromatography to generate a precipitate that blocks the test system and affects the liquid chromatography test, thereby improving the protection of the test system and the accuracy of subsequent tests.

[0058] Specifically, the equation for the reaction between the stannate ions and hydrogen ions in sodium stannate is as follows:

[0059] SnO 3 2- +2H + ===H 2 SnO 3 ↓

[0060] In some embodiments, the acidic neutralization solution includes an acid and a first diluent.

[0061] Furthermore, the acid is a non-oxidizing acid or an acid with low oxidizing property.

[0062] Specifically, the acid includes one or more of phosphoric acid, formic acid, and acetic acid. Specifically, the acetic acid can be glacial acetic acid.

[0063] In some embodiments, the acid is of analytical grade, for example, the concentration of phosphoric acid is above 85%, and the concentration of formic acid is above 80%.

[0064] In some embodiments, the first diluent includes water.

[0065] In some embodiments, in the acidic neutralizing solution, the volume ratio of the acid to the first diluent is (51-59):(21-29), for example, 51:29, 52:28, 53:27, 54:26, 55:25, 56:24, 57:23, 58:22, 59:21 or a range between any two ratios, etc. Within the volume ratio range, the concentration of the acidic neutralizing solution is appropriate, which is conducive to neutralizing the alkali in the electroplating solution and combining with sodium stannate to remove sodium stannate.

[0066] It can be understood that the dispersant may be a dispersant known in the art for dispersing graphene.

[0067] In some embodiments, the dispersant includes one or more of sulfonates, sulfates, and polyethers.

[0068] Specifically, the sulfonates include one or more of sodium polynaphthalene sulfonate and sodium dodecylbenzene sulfonate.

[0069] The sulfates include sodium lauryl sulfate.

[0070] The polyethers include alkylphenol polyoxyethylene ethers.

[0071] In some embodiments, in the electroplating solution, the mass concentration of the graphene is 0.5 g / L to 1.5 g / L, for example, 0.6 g / L, 0.8 g / L, 1 g / L, 1.2 g / L or a range between any two values.

[0072] In some embodiments, in the electroplating solution, the mass concentration of the sodium stannate is 100 g / L to 145 g / L, for example, 110 g / L, 120 g / L, 130 g / L, 140 g / L or a range between any two values.

[0073] In some embodiments, the electroplating solution further includes one or more of a metal salt and an alkali.

[0074] In some embodiments, the metal salt includes a copper salt. It is understood that the electroplating solution contains tin ions and copper ions, and a copper-tin alloy can be co-plated.

[0075] Furthermore, the copper salt includes one or more of cuprous cyanide, copper sulfate, copper chloride, and copper pyrophosphate.

[0076] In some embodiments, in the electroplating solution, the mass concentration of the copper salt is 5 g / L to 20 g / L, for example, 6 g / L, 8 g / L, 10 g / L, 12 g / L, 15 g / L, 18 g / L or a range between any two values.

[0077] In some embodiments, the alkali includes one or more of potassium hydroxide and sodium hydroxide. The addition of potassium hydroxide and sodium hydroxide can enhance the conductivity of the electroplating solution, making the current more evenly distributed in the plating solution; it can also make the plating layer more uniform and fine, and reduce defects and roughness in the plating layer.

[0078] In some embodiments, the mass concentration of the alkali in the electroplating solution is 5 g / L to 15 g / L, for example, 6 g / L, 8 g / L, 10 g / L, 12 g / L, or a range between any two values. It should be noted that when the alkali excessively affects the pH in the electroplating solution, the acidic neutralizing solution can also neutralize the excess alkali in the electroplating solution.

[0079] In some embodiments, the electroplating solution further comprises a solvent. Further, the solvent is selected from one or more of water, ethanol, isopropanol, N-methylpyrrolidone (NMP), dichloromethane, xylene, dichlorobenzene, ethylene glycol, and toluene.

[0080] In some embodiments, the volume ratio of the acidic neutralizing solution to the electroplating solution is (60-80):10, for example, 60:10, 65:10, 70:10, 75:10, or any range between two ratios. Within the volume ratio range, the acidic neutralizing solution is conducive to neutralizing the alkali in the electroplating solution and combining with sodium stannate to remove sodium stannate.

[0081] In some embodiments, the mixing of the acidic neutralization solution and the electroplating solution further comprises: adding a second diluent to obtain a mixed solution, and performing the first filtration on the mixed solution.

[0082] In some embodiments, the second diluent includes water.

[0083] In some embodiments, the volume ratio of the electroplating solution to the mixed solution is 10:(100-500), for example, it can be 10:150, 10:200, 10:250, 10:300, 10:350, 10:400, 10:450 or any range between two ratios. It should be noted that the use of the second diluent for dilution can protect the chromatographic column of the liquid chromatograph and make the chromatogram integral area reasonable, so that the test results are more accurate.

[0084] Exemplarily, the addition of the second diluent can be achieved by fixing the volume. When the plating solution is 10 mL and the acid neutralizing solution is 80 mL, the plating solution and the acid neutralizing solution are mixed, and then the second diluent is added to fix the volume to 100 mL to prepare a mixed solution.

[0085] In some embodiments, the mixing of the acidic neutralizing solution and the electroplating solution further includes stirring. Further, the stirring time is 20 minutes to 50 minutes, for example, 22 minutes, 25 minutes, 28 minutes, 30 minutes, 32 minutes, 35 minutes, 38 minutes, or a range between any two values. Within the time range, it is beneficial to fully mix the acidic neutralizing solution and the electroplating solution, and remove the generated stannic acid.

[0086] In some embodiments, the first filtering method comprises microporous membrane filtration.

[0087] It should be noted that the particle size of stannic acid precipitate is greater than 100 μm, which is much larger than the particle size of graphene. Therefore, the pore size of the microporous filter membrane can be selected according to the particle size of graphene in the electroplating solution and the accuracy of the existing detection device, so as to remove the graphene and other solid particles with larger particle sizes in the electroplating solution as much as possible, improve the accuracy of dispersant detection, and avoid the presence of graphene or other solid particles with larger particle sizes affecting the concentration of the dispersant.

[0088] In some embodiments, the sample to be tested includes the dispersant.

[0089] Second, see Figure 2 The present application also provides a method for testing a dispersant in a sample to be tested, comprising the following steps:

[0090] S21: providing a sample to be tested after being treated by the above-mentioned electroplating solution treatment method;

[0091] S22: Performing a liquid chromatography test on the sample to be tested to obtain the concentration of the dispersant.

[0092] The liquid chromatography is a method for achieving separation by causing the target substance in the test solution to undergo specific adsorption and desorption on the chromatographic column through different compositions and ratios of mobile phases, and then being detected and converted on a detector to form a chromatogram for quantitative analysis.

[0093] In some embodiments, the performing liquid chromatography test on the sample to be tested includes: performing a second filtration on the sample to be tested and then adding the sample to a chromatography bottle for liquid chromatography test.

[0094] In some embodiments, the second filtering method is a needle filter filtration. The needle filter can further filter out possible insoluble particles to protect the chromatographic column and improve the utilization rate of the liquid chromatograph.

[0095] In some embodiments, the mobile phase of the liquid chromatography test includes a mixture of methanol and phosphoric acid aqueous solution. It should be noted that the phosphoric acid aqueous solution is a solution formed by dissolving phosphoric acid in water, wherein the concentration of phosphoric acid can be 0.2 vol%, wherein vol% represents volume fraction.

[0096] Furthermore, in the mixed solution, the volume ratio of the methanol to the phosphoric acid aqueous solution is (25-60):(40-75), for example, it can be 25:75, 30:70, 35:65, 40:60, 45:55, 50:50, 55:45, 60:40 or a range between any two ratios.

[0097] In some embodiments, the flow rate of the mobile phase of the liquid chromatography test is 0.8 mL / min to 1.5 mL / min, for example, it can be 0.8 mL / min, 0.9 mL / min, 1 mL / min, 1.1 mL / min, 1.2 mL / min, 1.3 mL / min, 1.4 mL / min, 1.5 mL / min or a range between any two values.

[0098] In some embodiments, the wavelength of the ultraviolet detector of the liquid chromatography test is 300nm~345nm, for example, it can be 300nm, 302nm, 305nm, 308nm, 310nm, 312nm, 315nm, 318nm, 320nm, 322nm, 325nm, 328nm, 330nm, 332nm, 335nm, 338nm, 340nm, 342nm, 345nm or a range between any two values.

[0099] In some embodiments, the temperature of the column oven of the liquid chromatography test is 28°C to 35°C, for example, it can be 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C or a range between any two values.

[0100] In some embodiments, the elution time of the liquid chromatography test is 18 min to 45 min, for example, it can be 20 min, 25 min, 30 min, 35 min, 40 min or a range between any two values.

[0101] In this way, under the above-mentioned liquid chromatography test conditions, it is conducive to efficiently and accurately testing the concentration of the dispersant.

[0102] In some embodiments, the liquid chromatography test is high performance liquid chromatography. When using high performance liquid chromatography, the sample to be tested is injected into the chromatographic column and moves in the stationary phase by pressure. Due to the different interactions between different substances of the tested species and the stationary phase, different substances leave the chromatographic column in sequence, and different peak signals are obtained through the detector. Finally, the substances contained in the tested object are determined by analyzing and comparing these signals.

[0103] It should be noted that after the liquid chromatography test, a chromatogram can be obtained, and the concentration of the dispersant can be obtained by integrating the chromatogram. The concentration of the dispersant is the volume concentration of the dispersant.

[0104] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0105] Example 1

[0106] This embodiment provides a method for treating an electroplating solution, comprising:

[0107] Preparation of acidic neutralization solution: Measure 51 mL of phosphoric acid (analytical grade), dilute to 80 mL with water to obtain acidic neutralization solution;

[0108] Copper-tin alloy graphene electroplating solution: including dispersant sodium polynaphthalene sulfonate with a volume concentration of 20 mL / L, graphene with a mass concentration of 1 g / L, and sodium stannate with a mass concentration of 120 g / L;

[0109] Mixing reaction: In a fume hood, take 10 mL of copper-tin alloy graphene electroplating solution, slowly add 80 mL of prepared acid neutralization solution, then add ultrapure water and make up to 100 mL, and stir for 30 minutes;

[0110] Preparation of samples to be tested: The particle size distribution of graphene particles in the copper-tin alloy graphene electroplating solution is: D03=0.052μm, D10=0.063μm, D25=0.081μm, D50=0.489μm, D97=2.267μm. Since the minimum pore size of the existing microporous filter membrane is 0.05μm, a microporous filter membrane with a pore size of 0.05μm is selected to filter the solution after the above mixed reaction to remove the solid particles insoluble in water. The filtrate is the sample to be tested.

[0111] Accordingly, this embodiment also provides a method for testing a dispersant in a sample to be tested, comprising:

[0112] 1 mL of the above filtrate was filtered through a syringe filter and then added dropwise to a 1.5 mL chromatography bottle for liquid chromatography testing;

[0113] Liquid chromatography test conditions: mobile phase composition: V (methanol): V (0.2 vol% phosphoric acid aqueous solution) = 37:63, flow rate is 1 mL / min, UV detector wavelength is 311 nm, column oven temperature is 30°C, elution time is 20 min; after the test system is stable, 1 mL of filtrate is drawn for test analysis, and the injection volume is 35 μL.

[0114] Example 2

[0115] This embodiment provides a method for treating an electroplating solution, comprising:

[0116] Preparation of acidic neutralization solution: Measure 59 mL of phosphoric acid (analytical grade), dilute to 80 mL with water to obtain acidic neutralization solution;

[0117] Copper-tin alloy graphene electroplating solution: including dispersant sodium polynaphthalene sulfonate with a volume concentration of 20 mL / L, graphene with a mass concentration of 1 g / L, and sodium stannate with a mass concentration of 120 g / L;

[0118] Mixing reaction: In a fume hood, take 10 mL of copper-tin alloy graphene electroplating solution, slowly add 80 mL of prepared acid neutralization solution, then add ultrapure water and make up to 100 mL, and stir for 30 minutes;

[0119] Preparation of samples to be tested: The particle size distribution of graphene particles in the copper-tin alloy graphene electroplating solution is: D03=0.052μm, D10=0.063μm, D25=0.081μm, D50=0.489μm, D97=2.267μm. Since the minimum pore size of the existing microporous filter membrane is 0.05μm, a microporous filter membrane with a pore size of 0.05μm is selected to filter the solution after the above mixed reaction to remove the solid particles insoluble in water. The filtrate is the sample to be tested.

[0120] Accordingly, this embodiment also provides a method for testing a dispersant in a sample to be tested, comprising:

[0121] 1 mL of the above filtrate was filtered through a syringe filter and then added dropwise to a 1.5 mL chromatography bottle for liquid chromatography testing;

[0122] Liquid chromatography test conditions: mobile phase composition: V (methanol): V (0.2 vol% phosphoric acid aqueous solution) = 37:63, flow rate is 1 mL / min, UV detector wavelength is 311 nm, column oven temperature is 30°C, elution time is 20 min; after the test system is stable, 1 mL of filtrate is drawn for test analysis, and the injection volume is 35 μL.

[0123] Example 3

[0124] This embodiment provides a method for treating an electroplating solution, comprising:

[0125] Preparation of acidic neutralization solution: Measure 55 mL of glacial acetic acid (analytical grade), dilute to 80 mL with water to obtain acidic neutralization solution;

[0126] Copper-tin alloy graphene electroplating solution: including dispersant sodium polynaphthalene sulfonate with a volume concentration of 20 mL / L, graphene with a mass concentration of 1 g / L, and sodium stannate with a mass concentration of 120 g / L;

[0127] Mixing reaction: In a fume hood, take 10 mL of copper-tin alloy graphene electroplating solution, slowly add 80 mL of prepared acid neutralization solution, then add ultrapure water and make up to 100 mL, and stir for 30 minutes;

[0128] Preparation of samples to be tested: The particle size distribution of graphene particles in the copper-tin alloy graphene electroplating solution is: D03=0.052μm, D10=0.063μm, D25=0.081μm, D50=0.489μm, D97=2.267μm. Since the minimum pore size of the existing microporous filter membrane is 0.05μm, a microporous filter membrane with a pore size of 0.05μm is selected to filter the solution after the above mixed reaction to remove the solid particles insoluble in water. The filtrate is the sample to be tested.

[0129] Accordingly, this embodiment also provides a method for testing a dispersant in a sample to be tested, comprising:

[0130] 1 mL of the above filtrate was filtered through a syringe filter and then added dropwise to a 1.5 mL chromatography bottle for liquid chromatography testing;

[0131] Liquid chromatography test conditions: mobile phase composition: V (methanol): V (0.2 vol% phosphoric acid aqueous solution) = 37:63, flow rate is 1 mL / min, UV detector wavelength is 311 nm, column oven temperature is 30°C, elution time is 20 min; after the test system is stable, 1 mL of filtrate is drawn for test analysis, and the injection volume is 35 μL.

[0132] Example 4

[0133] This embodiment provides a method for treating an electroplating solution, comprising:

[0134] Preparation of acidic neutralization solution: Measure 55 mL of formic acid (analytical grade), dilute to 80 mL with water to obtain acidic neutralization solution;

[0135] Copper-tin alloy graphene electroplating solution: including dispersant sodium polynaphthalene sulfonate with a volume concentration of 20 mL / L, graphene with a mass concentration of 1 g / L, and sodium stannate with a mass concentration of 120 g / L;

[0136] Mixing reaction: In a fume hood, take 10 mL of copper-tin alloy graphene electroplating solution, slowly add 80 mL of prepared acid neutralization solution, then add ultrapure water and make up to 100 mL, and stir for 30 minutes;

[0137] Preparation of samples to be tested: The particle size distribution of graphene particles in the copper-tin alloy graphene electroplating solution is: D03=0.052μm, D10=0.063μm, D25=0.081μm, D50=0.489μm, D97=2.267μm. Since the minimum pore size of the existing microporous filter membrane is 0.05μm, a microporous filter membrane with a pore size of 0.05μm is selected to filter the solution after the above mixed reaction to remove the solid particles insoluble in water. The filtrate is the sample to be tested.

[0138] Accordingly, this embodiment also provides a method for testing a dispersant in a sample to be tested, comprising:

[0139] 1 mL of the above filtrate was filtered through a syringe filter and then added dropwise to a 1.5 mL chromatography bottle for liquid chromatography testing;

[0140] Liquid chromatography test conditions: mobile phase composition: V (methanol): V (0.2 vol% phosphoric acid aqueous solution) = 37:63, flow rate is 1 mL / min, UV detector wavelength is 311 nm, column oven temperature is 30°C, elution time is 20 min; after the test system is stable, 1 mL of filtrate is drawn for test analysis, and the injection volume is 35 μL.

[0141] The volume concentrations of the chromatograms of Examples 1 to 4 were calculated by integrating them. The results are shown in Table 1.

[0142] Table 1

[0143]

[0144] As can be seen from Table 1, after the sodium stannate in the plating solution is treated by the plating solution treatment method provided in the present application, the obtained sample to be tested is then subjected to liquid chromatography treatment, and the measured volume concentration of the dispersant has a high accuracy rate, and the sodium stannate is removed, thereby avoiding the sodium stannate in the plating solution from reacting with the mobile phase phosphoric acid in the liquid chromatography test to generate a precipitate that blocks the test system, thereby improving the protection of the test system and the accuracy of subsequent tests.

[0145] The technical solutions provided by the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for treating an electroplating solution, characterized in that: The steps include: Providing an acidic neutralizing solution and an electroplating solution, wherein the electroplating solution comprises sodium stannate, a dispersant and graphene; The acidic neutralization solution and the electroplating solution are mixed, and the precipitate is removed after a first filtration to obtain a sample to be tested.

2. The processing method according to claim 1, characterized in that: The acidic neutralization solution comprises an acid and a first diluent; and / or The dispersant includes one or more of sulfonates, sulfates, and polyethers; and / or The volume ratio of the acidic neutralization solution to the electroplating solution is (60-80):10; and / or The sample to be tested includes the dispersant.

3. The processing method according to claim 2, characterized in that: The acid comprises one or more of phosphoric acid, formic acid and acetic acid; and / or The first diluent comprises water; and / or The sulfonates include one or more of sodium polynaphthalene sulfonate and sodium dodecylbenzene sulfonate; and / or The sulfates include sodium lauryl sulfate; and / or The polyethers include alkylphenol polyoxyethylene ethers; and / or In the acidic neutralization solution, the volume ratio of the acid to the diluent is (51-59):(21-29).

4. The processing method according to claim 1, characterized in that: In the electroplating solution, the mass concentration of the graphene is 0.5 g / L to 1.5 g / L; and / or In the electroplating solution, the mass concentration of the sodium stannate is 100 g / L to 145 g / L; and / or The electroplating solution also includes one or more of a solvent, a metal salt, and an alkali.

5. The processing method according to claim 4, characterized in that: The solvent is selected from one or more of water, ethanol, isopropanol, N-methylpyrrolidone, dichloromethane, xylene, dichlorobenzene, ethylene glycol, and toluene; and / or The metal salt comprises a copper salt, and the copper salt comprises one or more of cuprous cyanide, copper sulfate, copper chloride, and copper pyrophosphate; and / or In the electroplating solution, the mass concentration of the copper salt is 5 g / L to 20 g / L; and / or The alkali comprises one or more of potassium hydroxide and sodium hydroxide; and / or In the electroplating solution, the mass concentration of the alkali is 5 g / L to 15 g / L.

6. The processing method according to claim 1, characterized in that: The mixing of the acidic neutralization solution and the electroplating solution further comprises: adding a second diluent to obtain a mixed solution, and performing the first filtration on the mixed solution; wherein, The second diluent comprises water; and / or The volume ratio of the electroplating solution to the mixed solution is 10:(100-500); and / or The method of adding the second diluent includes fixing the volume.

7. The processing method according to claim 1, characterized in that: After the acidic neutralization solution and the electroplating solution are mixed, stirring is further included, and the stirring time is 20 minutes to 50 minutes; and / or The first filtering method includes microporous membrane filtration.

8. A method for testing a dispersant in a sample to be tested, characterized in that: The steps include: Providing a sample to be tested after being treated by the electroplating solution treatment method according to any one of claims 1 to 7; The sample to be tested is subjected to a liquid chromatography test to obtain the concentration of the dispersant.

9. The testing method according to claim 8, characterized in that: The liquid chromatography test on the sample to be tested comprises: after the sample to be tested is subjected to a second filtration, adding the sample to a chromatographic bottle for liquid chromatography test; wherein the second filtration method is needle filter filtration; and / or The concentration of the dispersant is the volume concentration of the dispersant.

10. The testing method according to any one of claims 8 to 9, characterized in that: The mobile phase of the liquid chromatography test comprises a mixture of methanol and an aqueous phosphoric acid solution; wherein the volume ratio of the methanol to the aqueous phosphoric acid solution is (25-60): (40-75); and / or The flow rate of the mobile phase of the liquid chromatography test is 0.8 mL / min to 1.5 mL / min; and / or The wavelength of the ultraviolet detector of the liquid chromatography test is 300nm to 345nm; and / or The temperature of the column oven of the liquid chromatography test is 28°C to 35°C; and / or The elution time of the liquid chromatography test is 18 min to 45 min.