Infrared glass wide-angle multiband optical window and manufacturing method thereof
By alternately deposition of YBF3 film and ZnS film on the optical window and using AF film on the outer surface, the multi-band transmittance and pollution problems of traditional optical windows are solved, high transmittance and self-cleaning ability are achieved, and service life is extended .
Patent Information
- Application Number
- CN202411175960.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Traditional optical windows are difficult to meet the needs of multi-band high transmittance, and are susceptible to pollution from dust, oil and other pollution, resulting in frequent maintenance and affecting optical performance.
The YBF3 film and ZnS film of a specific thickness are alternately evaporated on the substrate, and the AF film is used instead of the ZnS film on the outer surface of the tenth YBF3 film. The vacuum deposition is performed through an evaporation coating machine with an RF ion source to optimize the film layer. The structure is to improve light transmittance and water drop angle, and to prevent pollution and dust.
The light transmittance is greater than 85% in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band, and has self-cleaning ability, extending the service life of the optical window.
Smart Images

Figure CN119045094A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of optical coating, and in particular to an infrared glass large-angle multi-band optical window and a manufacturing method thereof. Background Art
[0002] With the development of modern optical technology, the demand for optical windows with high transmittance is growing, especially in high-end application fields such as military, aerospace, monitoring and optical instruments. Traditional optical window materials can only achieve high transmittance for specific bands and it is difficult to meet the demand for multi-band transmittance. In addition, optical windows are easily contaminated by dust, oil and other pollutants during use, which affects the optical performance. Therefore, they need to be cleaned frequently, which increases the maintenance cost. Summary of the invention
[0003] In order to improve the problem that optical windows in related technologies are difficult to meet the requirements of multi-band high transmittance and are easily contaminated, the present application provides an infrared glass large-angle multi-band optical window and a manufacturing method thereof.
[0004] In the first aspect, the present application provides an infrared glass large-angle multi-band optical window adopts the following technical solution: a multi-band optical window comprises a substrate, and the upper and lower surfaces of the substrate are sequentially evaporated with a first YBF 3 Film, first ZnS film, second YBF 3 film, the second ZnS film, the third YBF 3 film, the third ZnS film, the fourth YBF 3 Film, fourth ZnS film, fifth YBF 3 Film, fifth ZnS film, sixth YBF 3 Film, the sixth ZnS film, the seventh YBF 3 Film, seventh ZnS film, eighth YBF 3 Film, the eighth ZnS film, the ninth YBF 3 Film, ninth ZnS film, tenth YBF 3 Film and AF film; Among them, the first YBF 3 The thickness of the film is 48.78±2%nm, the thickness of the first ZnS film is 23.59±2%nm, and the thickness of the second YBF 3 The thickness of the first ZnS film is 109.07±2% nm, the thickness of the second ZnS film is 27.14±2% nm, and the thickness of the third YBF 3 The thickness of the film is 43.53±2% nm, the thickness of the third ZnS film is 177.33±2% nm, and the thickness of the fourth YBF 3 The thickness of the film is 41.91±2% nm, the thickness of the fourth ZnS film is 26.77±2% nm, and the thickness of the fifth YBF3 The thickness of the film is 84.69±2% nm, the thickness of the fifth ZnS film is 9.79±2% nm, and the thickness of the sixth YBF 3 The thickness of the film is 89.95±2% nm, the thickness of the sixth ZnS film is 17.39±2% nm, and the thickness of the seventh YBF 3 The thickness of the film is 78.84±2% nm, the thickness of the seventh ZnS film is 18.65±2% nm, and the thickness of the eighth YBF 3 The thickness of the film is 311.74±2% nm, the thickness of the eighth ZnS film is 11.10±2% nm, and the thickness of the ninth YBF 3 The thickness of the film is 103.16±2% nm, the thickness of the ninth ZnS film is 7.74±2% nm, and the thickness of the tenth YBF 3 The thickness of the film was 167.60±2% nm, and the thickness of the AF film was 20±50% nm.
[0005] In this application, YBF with a specific thickness is alternately evaporated on the substrate. 3 Film and ZnS film can obtain an optical window with a light transmittance greater than 85% in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band (within the range of 0° to 60°). 3 The outer surface of the membrane uses an AF film of specific thickness instead of the ZnS film, which can increase the water drop angle of the optical window, which is conducive to obtaining an optical window with good self-cleaning ability, anti-fouling and dust-proof, and not easy to be contaminated. It does not require frequent maintenance and can prevent scratches during maintenance from affecting the light transmittance of the optical window in a specific band. It is beneficial to maintain the stability of the light transmittance of the optical window in a specific band and extend the service life of the optical window.
[0006] In some specific embodiments, the substrate is a ZnS substrate or a ZnSe substrate.
[0007] The substrate of the optical window of the present application adopts a ZnS substrate or a ZnSe substrate, wherein both ZnS and ZnSe have a high light transmittance in the infrared band, and cooperate with the above-mentioned vapor-deposited film layer to obtain an optical window with a light transmittance greater than 85% in the 0.5μm-1μm band, the 3.7μm-4.8μm band, and the 7.7μm-12μm band (within the range of 0° to 60°). In addition, both ZnS and ZnSe have excellent chemical stability, which is conducive to improving the stability of the optical window.
[0008] In some specific embodiments, the multi-band optical window simultaneously satisfies that the light transmittance in the range of 0° to 60° in the 0.5 μm-1 μm band, the 3.7 μm-4.8 μm band, and the 7.7 μm-12 μm band is greater than 85%.
[0009] In some specific embodiments, the water drop angle of the multi-band optical window is 110-120°.
[0010] In the present application, the water drop angle of the multi-band optical window is within the range of 110-120°, which can improve the multi-band optical window and the tenth YBF while obtaining an optical window with good self-cleaning ability, anti-fouling and dust-proof, and not easy to be polluted. 3 The bonding strength of the film.
[0011] In a second aspect, the present application provides a method for manufacturing a multi-band optical window, the manufacturing method adopts the following technical solution: A method for manufacturing a multi-band optical window comprises the following steps: Prepare coating material YBF 3 , ZnS and AF pills; The first YBF was vacuum-deposited on the upper and lower surfaces of the substrate using an evaporation coating machine with an RF ion source. 3 Film, first ZnS film, second YBF 3 film, the second ZnS film, the third YBF 3 film, the third ZnS film, the fourth YBF 3 Film, fourth ZnS film, fifth YBF 3 Film, fifth ZnS film, sixth YBF 3 Film, the sixth ZnS film, the seventh YBF 3 Film, seventh ZnS film, eighth YBF 3 Film, the eighth ZnS film, the ninth YBF 3 Film, ninth ZnS film, tenth YBF 3 Film and AF film.
[0012] In this application, an evaporation coating machine with an RF ion source is used to evaporate YBF 3 Film layer, ZnS film layer and AF film layer, compared with the Hall ion source, the RF ion source has greater energy, which is beneficial to optimize the lattice structure of each film layer and obtain an optical window with a light transmittance greater than 85% in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band (within the range of 0° to 60°).
[0013] In some specific embodiments, the first YBF is evaporated 3 Film ~ 10th YBF 3During film deposition, the screen grid voltage of the RF ion source is controlled to be 500±10%V, the screen grid current is 350±10%A, the accelerating electrode voltage is 500±10%V, the RF power is 205±10%KW, and the argon gas flow rate is 20±10%sccm; the emitter voltage of the RF neutralizer is controlled to be 150±10%V, the emitter current is 2±10%A, the maintaining electrode voltage is 100±10%V, the maintaining electrode current is 1500±10%A, and the argon gas flow rate is 10±10%sccm.
[0014] Evaporation YBF 3 When coating, controlling the parameters of the RF ion source and RF neutralizer within the above range is beneficial to optimize the YBF 3 The lattice structure of the film reduces YBF 3 The film layer absorbs specific light, so that the multi-band optical window can simultaneously meet the light transmittance of more than 85% in the range of 0° to 60° in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band.
[0015] In some specific embodiments, the first YBF is evaporated 3 Film ~ 10th YBF 3 When filming, control YBF 3 The deposition rate of the film layer is 5±2% A / s.
[0016] Evaporation YBF 3 When the membrane is used, control the first YBF 3 Film ~ 10th YBF 3 YBF in membrane 3 The deposition rate of the film layer is within the range of 5±2% A / s, which is conducive to further improving the first YBF 3 Film ~ 10th YBF 3 The uniformity of film deposition not only obtains optical windows with light transmittance greater than 85% in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band (within the range of 0° to 60°), but also further promotes the firm bonding between the film layers, which is beneficial to extending the service life of the multi-band optical window.
[0017] In some specific embodiments, when the first to ninth ZnS films are evaporated, the screen grid voltage of the RF ion source is controlled to be 1100±10%V, the screen grid current is 800±10%A, the accelerating electrode voltage is 700±10%V, the RF power is 430±10%KW, the argon flow rate is 100±10%sccm, and the oxygen flow rate is 60±10%sccm; the emitter voltage of the RF neutralizer is controlled to be 150±10%V, the emitter current is 2±10%A, the maintaining electrode voltage is 100±10%V, the maintaining electrode current is 1500±10%A, and the argon flow rate is 10±10%sccm.
[0018] When evaporating the ZnS film, controlling the parameters of the RF ion source and the RF neutralizer within the above range is beneficial to optimizing the lattice structure of the ZnS film, reducing the absorption of specific light by the ZnS film, and allowing the multi-band optical window to simultaneously meet the light transmittance of more than 85% in the range of 0° to 60° in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band.
[0019] In some specific implementations, when evaporating the first to ninth ZnS films, the deposition rate of the ZnS film layer is controlled to be 3±2% A / s.
[0020] When evaporating the ZnS film, controlling the deposition rate of the ZnS film layer in the first ZnS film to the ninth ZnS film within the range of 3±2% A / s is beneficial to further improve the deposition uniformity of the first ZnS film to the ninth ZnS film, while obtaining optical windows with light transmittance greater than 85% in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band (within the range of 0° to 60°), further promoting the firm bonding between the film layers, which is beneficial to extending the service life of the multi-band optical window.
[0021] In some specific embodiments, when evaporating the AF film, the evaporation rate of the AF pellets is controlled to be >6A / s.
[0022] In some specific embodiments, the vacuum degree of the evaporation coating machine with RF ion source is controlled to be 3.0*10 -5 torr-2.0*10 -5 torr, and the temperature was controlled at 150±10%℃.
[0023] In the present application, controlling the vacuum degree and temperature of the evaporation coating machine with an RF ion source within the above range is conducive to stabilizing the deposition rate and obtaining a uniform and dense film layer structure.
[0024] In summary, this application at least includes the following beneficial technical effects: In this application, YBF with a specific thickness is alternately evaporated on the substrate. 3 Film and ZnS film can obtain an optical window with a light transmittance greater than 85% in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band (within the range of 0° to 60°). 3 The outer surface of the membrane uses an AF film of specific thickness instead of the ZnS film, which can increase the water drop angle of the optical window, which is conducive to obtaining an optical window with good self-cleaning ability, anti-fouling and dust-proof, and not easy to be contaminated. It does not require frequent maintenance and can prevent scratches during maintenance from affecting the light transmittance of the optical window in a specific band. It is beneficial to maintain the stability of the light transmittance of the optical window in a specific band and extend the service life of the optical window. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a structural schematic diagram of an infrared glass large-angle multi-band optical window according to an embodiment of the present application.
[0026] Figure 2 It is a curve chart of the light transmittance of the infrared glass wide-angle multi-band optical window in Example 3 at 0°, 10°, 20°, 30°, 40°, 50°, and 60° in the 0.5μm-1μm band.
[0027] Figure 3 It is a curve chart of the light transmittance of the infrared glass wide-angle multi-band optical window in Example 3 at 0°, 10°, 20°, 30°, 40°, 50°, and 60° in the 3.7μm-4.8μm band.
[0028] Figure 4 It is a curve chart of the light transmittance of the infrared glass wide-angle multi-band optical window in Example 3 at 0°, 10°, 20°, 30°, 40°, 50°, and 60° in the 7.7μm-12μm band.
[0029] Figure 5 It is a curve chart of the light transmittance of the infrared glass wide-angle multi-band optical window in Example 4 at 0°, 10°, 20°, 30°, 40°, 50°, and 60° in the 0.5μm-1μm band.
[0030] Figure 6 It is a curve chart of the light transmittance of the infrared glass wide-angle multi-band optical window in Example 4 at 0°, 10°, 20°, 30°, 40°, 50°, and 60° in the 3.7μm-4.8μm band.
[0031] Figure 7It is a curve chart of the light transmittance of the infrared glass wide-angle multi-band optical window in Example 4 in the 7.7μm-12μm band at 0°, 10°, 20°, 30°, 40°, 50°, and 60°.
[0032] Figure 8 It is a comparison chart of the light transmittance curve of the optical window in Example 1 at 0.5μm-1μm band at 0° (dark color) and the light transmittance curve of the infrared glass wide-angle multi-band optical window in Example 4 at 0.5μm-1μm band at 0° (light color).
[0033] Fig. 9 It is a comparison chart of the light transmittance curve of the optical window in Example 2 at 0.5μm-1μm band at 0° (dark color) and the light transmittance curve of the infrared glass wide-angle multi-band optical window in Example 4 at 0.5μm-1μm band at 0° (light color).
[0034] Fig.10 It is a comparison chart of the light transmittance curve of the optical window in Example 3 at 0.5μm-1μm band at 0° (dark color) and the light transmittance curve of the infrared glass wide-angle multi-band optical window in Example 4 at 0.5μm-1μm band at 0° (light color).
[0035] Fig.11 It is a comparison chart of the light transmittance curve of the optical window in Example 4 at 0.5μm-1μm band at 0° (dark color) and the light transmittance curve of the infrared glass wide-angle multi-band optical window in Example 4 at 0.5μm-1μm band at 0° (light color).
[0036] Fig.12 It is a comparison chart of the light transmittance curve of the optical window in Example 5 at 0.5μm-1μm band at 0° (dark color) and the light transmittance curve of the infrared glass wide-angle multi-band optical window in Example 4 at 0.5μm-1μm band at 0° (light color).
[0037] Fig.13 It is a comparison chart of the light transmittance curve of the optical window in Example 6 at 0.5μm-1μm band at 0° (dark color) and the light transmittance curve of the infrared glass wide-angle multi-band optical window in Example 4 at 0.5μm-1μm band at 0° (light color).
[0038] Fig.14 It is a comparison chart of the light transmittance curve of the optical window in Example 7 at 0° in the 0.5μm-1μm band (dark color) and the light transmittance curve of the infrared glass wide-angle multi-band optical window in Example 4 at 0° in the 0.5μm-1μm band (light color).
[0039] Fig.15It is a comparison chart of the light transmittance curve of the optical window in Example 8 at 0.5μm-1μm band at 0° (dark color) and the light transmittance curve of the infrared glass wide-angle multi-band optical window in Example 4 at 0.5μm-1μm band at 0° (light color).
[0040] Description of reference numerals: 1. Base material; 01. First YBF 3 Film; 02, first ZnS film; 03, second YBF 3 Film; 04, second ZnS film; 05, third YBF 3 Film; 06, third ZnS film; 07, fourth YBF 3 Film; 08, fourth ZnS film; 09, fifth YBF 3 Film; 10, fifth ZnS film; 11, sixth YBF 3 Film; 12, sixth ZnS film; 13, seventh YBF 3 Film; 14, seventh ZnS film; 15, eighth YBF 3 Film; 16, the eighth ZnS film; 17, the ninth YBF 3 Film; 18, ninth ZnS film; 19, tenth YBF 3 Film; 20, AF film. DETAILED DESCRIPTION
[0041] The following is a further description of this application in conjunction with specific experiments: Example
[0042] [Example 1] An infrared glass large-angle multi-band optical window comprises a ZnS substrate, and a first YBF layer with a thickness of 47.8044 nm is sequentially deposited on the upper and lower surfaces of the ZnS substrate from the inside to the outside. 3 Film 01, first ZnS film with a thickness of 23.1182nm, 02, second YBF film with a thickness of 106.8886nm 3 film 03, a second ZnS film 04 with a thickness of 26.5972nm, a third YBF film with a thickness of 42.5972nm 3 film 05, a third ZnS film 06 with a thickness of 173.7834 nm, a fourth YBF film with a thickness of 41.0718 nm 3 film 07, a fourth ZnS film 08 with a thickness of 26.2346 nm, a fifth YBF film with a thickness of 82.9962 nm 3 film 09, a fifth ZnS film 10 with a thickness of 9.5942 nm, a sixth YBF film with a thickness of 88.151 nm 3 film 11, a sixth ZnS film 12 with a thickness of 17.0422 nm, a seventh YBF film with a thickness of 77.2632 nm3 film 13, a seventh ZnS film 14 with a thickness of 18.277 nm, an eighth YBF film 15 with a thickness of 305.5052 nm 3 film 15, an eighth ZnS film 16 with a thickness of 10.878 nm, and a ninth YBF film 10 with a thickness of 101.0968 nm. 3 film 17, a ninth ZnS film 18 with a thickness of 7.5852 nm, a tenth YBF film 164.248 nm 3 film 19 and an AF film 20 having a thickness of 25 nm.
[0043] In this embodiment, the method for manufacturing the infrared glass large-angle multi-band optical window includes the following steps: S1. Prepare coating material YBF 3 , ZnS and AF pills; S2, using an evaporation coating machine with an RF ion source to vacuum-deposit the first YBF on the upper and lower surfaces of the ZnS substrate 3 Film 01, first ZnS film 02, second YBF 3 Film 03, second ZnS film 04, third YBF 3 Film 05, third ZnS film 06, fourth YBF 3 Film 07, fourth ZnS film 08, fifth YBF 3 Film 09, fifth ZnS film 10, sixth YBF 3 Film 11, sixth ZnS film 12, seventh YBF 3 Film 13, seventh ZnS film 14, eighth YBF 3 Film 15, eighth ZnS film 16, ninth YBF 3 Film 17, ninth ZnS film 18, tenth YBF 3 Film 19 and AF film 20; Specifically, the first YBF is evaporated 3 Film ~ 10th YBF 3 During the membrane process, control YBF 3 The deposition rate of the film layer is 5.1A / s; more specifically, the vacuum degree of the evaporation coating machine with RF ion source is controlled to 2.0*10 -5 torr, temperature controlled at 135°C, screen grid voltage of RF ion source controlled at 550V, screen grid current controlled at 385A, accelerating electrode voltage controlled at 550V, RF power controlled at 225.5KW, argon gas flow rate controlled at 22sccm, emitter voltage of RF neutralizer controlled at 165V, emitter current controlled at 2.2A, sustaining electrode voltage controlled at 110V, sustaining electrode current controlled at 1650A, argon gas flow rate controlled at 11sccm; Specifically, during the deposition of the first ZnS film to the ninth ZnS film, the deposition rate of the ZnS film layer is controlled to be 3.06 A / s; more specifically, the vacuum degree of the evaporation coating machine with the RF ion source is controlled to be 2.0*10 -5 torr, the temperature was controlled at 135°C, the screen grid voltage of the RF ion source was controlled to be 1210V, the screen grid current was 880A, the accelerating electrode voltage was 770V, the RF power was 473KW, the argon flow rate was 110sccm, and the oxygen flow rate was 66sccm; the emitter voltage of the RF neutralizer was controlled to be 165V, the emitter current was 2.2A, the maintaining electrode voltage was 110V, the maintaining electrode current was 1650A, and the argon flow rate was 11sccm.
[0044] Specifically, when evaporating the AF film, the evaporation rate of the AF pills was controlled to be 6.5 A / s.
[0045] [Example 2] An infrared glass large-angle multi-band optical window comprises a ZnSe substrate, and the upper and lower surfaces of the ZnSe substrate are sequentially evaporated with a first YBF layer having a thickness of 49.7556 nm from the inside to the outside. 3 Film 01, first ZnS film with a thickness of 24.0618nm, 02, second YBF film with a thickness of 111.2514nm 3 film 03, a second ZnS film 04 with a thickness of 27.6828 nm, a third YBF film with a thickness of 44.4006 nm 3 film 05, a third ZnS film 06 with a thickness of 180.8766 nm, a fourth YBF film with a thickness of 42.7482 nm 3 film 07, a fourth ZnS film 08 with a thickness of 27.3054 nm, a fifth YBF film with a thickness of 86.3838 nm 3 film 09, a fifth ZnS film 10 with a thickness of 9.9858 nm, a sixth YBF film with a thickness of 91.749 nm 3 film 11, a sixth ZnS film 12 with a thickness of 17.7378 nm, a seventh YBF film with a thickness of 80.4168 nm 3 film 13, a seventh ZnS film 14 with a thickness of 19.023 nm, an eighth YBF film 15 with a thickness of 317.9748 nm 3 film 15, an eighth ZnS film 16 with a thickness of 11.322 nm, and a ninth YBF film 105.2232 nm. 3 film 17, a ninth ZnS film 18 with a thickness of 7.8948 nm, a tenth YBF film 19 with a thickness of 170.952 nm 3 film 19 and an AF film 20 having a thickness of 15 nm.
[0046] In this embodiment, the method for making the infrared glass wide-angle multi-band optical window is different from the method for making it in [Example 1] in that: Specifically, the first YBF is evaporated 3 Film ~ 10th YBF 3 During the membrane process, control YBF 3 The deposition rate of the film layer is 4.9A / s; more specifically, the vacuum degree of the evaporation coating machine with RF ion source is controlled to 3.0*10 -5 torr, temperature controlled at 135°C, screen grid voltage of RF ion source controlled at 450V, screen grid current controlled at 315A, accelerating electrode voltage controlled at 450V, RF power controlled at 184.5KW, argon gas flow rate controlled at 18sccm, emitter voltage of RF neutralizer controlled at 135V, emitter current controlled at 1.8A, sustaining electrode voltage controlled at 90V, sustaining electrode current controlled at 1350A, argon gas flow rate controlled at 9sccm; Specifically, during the deposition of the first ZnS film to the ninth ZnS film, the deposition rate of the ZnS film layer is controlled to be 2.94 A / s; more specifically, the vacuum degree of the evaporation coating machine with the RF ion source is controlled to be 3.0*10 -5 torr, the temperature was controlled at 135°C, the screen grid voltage of the RF ion source was controlled to be 990V, the screen grid current was 720A, the accelerating electrode voltage was 630V, the RF power was 387KW, the argon gas flow rate was 90sccm, and the oxygen flow rate was 54sccm; the emitter voltage of the RF neutralizer was controlled to be 135V, the emitter current was 1.8A, the maintaining electrode voltage was 90V, the maintaining electrode current was 1350A, and the argon gas flow rate was 9sccm.
[0047] Specifically, when evaporating the AF film, the evaporation rate of the AF pills was controlled to be 7.5 A / s.
[0048] [Example 3] An infrared glass large-angle multi-band optical window comprises a ZnS substrate, and the upper and lower surfaces of the ZnS substrate are sequentially evaporated with a first YBF layer of 48.78 nm from the inside to the outside. 3 Film 01, first ZnS film with a thickness of 23.59 nm, 02, second YBF film with a thickness of 109.07 nm 3 film 03, a second ZnS film 04 with a thickness of 27.14 nm, and a third YBF film with a thickness of 43.53 nm. 3 film 05, a third ZnS film 06 with a thickness of 177.33 nm, a fourth YBF film with a thickness of 41.91 nm 3 film 07, a fourth ZnS film 08 with a thickness of 26.77 nm, a fifth YBF film with a thickness of 84.69 nm 3film 09, a fifth ZnS film 10 with a thickness of 9.79 nm, a sixth YBF film with a thickness of 89.95 nm 3 film 11, a sixth ZnS film 12 with a thickness of 17.39 nm, a seventh YBF film 13 with a thickness of 78.84 nm 3 film 13, a seventh ZnS film 14 with a thickness of 18.65 nm, an eighth YBF film 15 with a thickness of 311.74 nm 3 film 15, an eighth ZnS film 16 with a thickness of 11.10 nm, and a ninth YBF film 103.16 nm in thickness. 3 film 17, a ninth ZnS film 18 with a thickness of 7.74 nm, a tenth YBF film 167.60 nm 3 film 19 and an AF film 20 having a thickness of 20 nm.
[0049] In this embodiment, the method for making the infrared glass large-angle multi-band optical window is different from that in [Example 1] in that: Specifically, the first YBF is evaporated 3 Film ~ 10th YBF 3 During the membrane process, control YBF 3 The deposition rate of the film layer is 5A / s; more specifically, the vacuum degree of the evaporation coating machine with RF ion source is controlled to 2.5*10 -5 torr, the temperature was controlled at 135°C, the screen grid voltage of the RF ion source was controlled to be 500V, the screen grid current was 350A, the accelerating electrode voltage was 500V, the RF power was 205KW, the argon gas flow rate was 20sccm, the emitter voltage of the RF neutralizer was controlled to be 150V, the emitter current was 2A, the sustaining electrode voltage was 100V, the sustaining electrode current was 1500A, and the argon gas flow rate was 10sccm; Specifically, during the deposition of the first ZnS film to the ninth ZnS film, the deposition rate of the ZnS film layer is controlled to be 3A / s; more specifically, the vacuum degree of the evaporation coating machine with the RF ion source is controlled to be 2.5*10 -5 torr, the temperature was controlled at 135°C, the screen grid voltage of the RF ion source was controlled to be 1100V, the screen grid current was 800A, the accelerating electrode voltage was 700V, the RF power was 430KW, the argon gas flow rate was 100sccm, and the oxygen flow rate was 60sccm; the emitter voltage of the RF neutralizer was controlled to be 150V, the emitter current was 2A, the maintaining electrode voltage was 100V, the maintaining electrode current was 1500A, and the argon gas flow rate was 10sccm.
[0050] Specifically, when evaporating the AF film, the evaporation rate of the AF pills was controlled to be 7.0 A / s.
[0051] [Example 4] An infrared glass large-angle multi-band optical window is different from [Example 3] in that the substrate 1 is different. In this embodiment, the substrate 1 is a ZnSe substrate.
[0052] Comparative Example [Comparative Example 1] An optical window, which differs from [Example 4] in that: the third YBF is not evaporated 3 Membrane 05.
[0053] [Comparative Example 2] An optical window, which differs from [Example 4] in that: the third YBF 3 The evaporated thickness of film 05 is 63.53 nm.
[0054] [Comparative Example 3] An optical window, which differs from [Example 4] in that the fifth YBF is not evaporated 3 Film 09.
[0055] [Comparative Example 4] An optical window, which differs from [Example 4] in that: the fifth YBF 3 The vapor-deposited thickness of Film 09 was 19.79 nm.
[0056] [Comparative Example 5] An optical window, which is different from [Example 4] in that: the eighth YBF is not evaporated 3 Membrane 15.
[0057] [Comparative Example 6] An optical window, which differs from [Example 4] in that: the eighth YBF 3 The vapor-deposited thickness of the film 15 was 321.74 nm.
[0058] [Comparative Example 7] An optical window, which differs from [Example 4] in that: the ninth YBF is not evaporated 3 Membrane 17.
[0059] [Comparative Example 8] An optical window, which differs from [Example 4] in that: the ninth YBF 3 The vapor-deposited thickness of the film 17 was 113.16 nm.
[0060] [Comparative Example 9] An infrared glass large-angle multi-band optical window, which differs from [Example 4] in that no AF film is evaporated.
[0061] Performance testing 1. Light transmittance: The light transmittance of the infrared glass wide-angle multi-band optical window in Examples 1-4 and Comparative Example 9 in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band was tested using a Fourier infrared tester, wherein the test angle range was 0°-60°, the light transmittance was tested every 10°, and the results were recorded in Table 1 below. In addition, the light transmittance of the optical window in Comparative Examples 1-8 was tested in the 0.5μm-1μm band at 0°. When the light transmittance did not meet the light transmittance greater than 85%, the light transmittance of other bands was not tested, and the results were recorded in Table 2 below.
[0062] 2. Water drop angle: The water drop angle of the infrared glass large-angle multi-band optical window prepared in each embodiment and comparative example was tested using a water drop angle tester, and the results were recorded in Table 3 below.
[0063] Table 1 Table 2 Table 3 Sample Water drop angle Example 1 110°-120° Example 2 110°-120° Example 3 110°-120° Example 4 110°-120° Comparative Example 1 110°-120° Comparative Example 2 110°-120° Comparative Example 3 110°-120° Comparative Example 4 110°-120° Comparative Example 5 110°-120° Comparative Example 6 110°-120° Comparative Example 7 110°-120° Comparative Example 8 110°-120° Comparative Example 9 35°-45° According to the test results in Example 4, Comparative Examples 1-8 and Table 1-2, the light transmittance of the infrared glass wide-angle multi-band optical window in the 0.5μm-1μm band, 3.7μm-4.8μm band, and 7.7μm-12μm band (within the range of 0° to 60°) is greater than 85%, which depends on the coordination of the film layer structure and the film layer thickness, neither of which can be missing.
[0064] According to the test results in Example 4, Comparative Example 9 and Table 3, it can be seen that the outermost layer of the infrared glass wide-angle multi-band optical window is provided with an AF film of a specific film thickness, which can increase the water drop angle of the infrared glass wide-angle multi-band optical window, so that the infrared glass wide-angle multi-band optical window obtains an optical window with a water drop angle within the range of 110-120°, good self-cleaning ability, anti-fouling and dust-proof, and not easy to be polluted.
[0065] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A multi-band optical window, characterized in that: The invention comprises a substrate (1), wherein the upper and lower surfaces of the substrate (1) are sequentially deposited with a first YBF3 film (01) with a thickness of 48.78±2% nm, a first ZnS film (02) with a thickness of 23.59±2% nm, a second YBF3 film (03) with a thickness of 109.07±2% nm, a second ZnS film (04) with a thickness of 27.14±2% nm, a third YBF3 film (05) with a thickness of 43.53±2% nm, a third ZnS film (06) with a thickness of 177.33±2% nm, a fourth YBF3 film (07) with a thickness of 41.91±2% nm, a fourth ZnS film (08) with a thickness of 26.77±2% nm, a fifth YBF3 film (09) with a thickness of 84.69±2% nm, and a fifth ZnS film (010) with a thickness of 9.79 ±2% nm, a fifth ZnS film (10) with a thickness of 89.95±2% nm, a sixth YBF3 film (11) with a thickness of 17.39±2% nm, a seventh YBF3 film (13) with a thickness of 78.84±2% nm, a seventh ZnS film (14) with a thickness of 18.65±2% nm, an eighth YBF3 film (15) with a thickness of 311.74±2% nm, an eighth ZnS film (16) with a thickness of 11.10±2% nm, a ninth YBF3 film (17) with a thickness of 103.16±2% nm, a ninth ZnS film (18) with a thickness of 7.74±2% nm, a tenth YBF3 film (19) with a thickness of 167.60±2% nm, and an AF film (20) with a thickness of 20±50% nm.
2. A multi-band optical window according to claim 1, characterized in that: The substrate (1) is a ZnS substrate or a ZnSe substrate.
3. A multi-band optical window according to claim 1, characterized in that: The multi-band optical window simultaneously satisfies that the light transmittance in the range of 0°~60° in the 0.5μm-1μm band, the 3.7μm-4.8μm band, and the 7.7μm-12μm band is greater than 85%.
4. The multi-band optical window according to claim 1, characterized in that: The water drop angle of the multi-band optical window is 110-120°.
5. A method for manufacturing a multi-band optical window according to any one of claims 1 to 4, characterized in that: The following steps are involved: Prepare coating materials ZnS, YbF3 and AF pellets; The upper and lower surfaces of the substrate (1) are vacuum coated in turn using an evaporation coating machine with an RF ion source. The first YBF3 film (01), the first ZnS film (02), the second YBF3 film (03), the second ZnS film (04), the third YBF3 film (05), the third ZnS film (06), the fourth YBF3 film (07), the fourth ZnS film (08), the fifth YBF3 film (09), the fifth ZnS film (10), the sixth YBF3 film (11), the sixth ZnS film (12), the seventh YBF3 film (13), the seventh ZnS film (14), the eighth YBF3 film (15), the eighth ZnS film (16), the ninth YBF3 film (17), the ninth ZnS film (18), the tenth YBF3 film (19) and the AF film (20) are evaporated.
6. The method for manufacturing a multi-band optical window according to claim 5, characterized in that: When evaporating the first to tenth YBF3 films, the screen grid voltage of the RF ion source is controlled to be 500±10%V, the screen grid current is 350±10%A, the accelerating electrode voltage is 500±10%V, the RF power is 205±10%KW, and the argon gas flow rate is 20±10%sccm; the emitter voltage of the RF neutralizer is controlled to be 150±10%V, the emitter current is 2±10%A, the maintaining electrode voltage is 100±10%V, the maintaining electrode current is 1500±10%A, and the argon gas flow rate is 10±10%sccm.
7. The method for manufacturing a multi-band optical window according to claim 5, characterized in that: When evaporating the first to tenth YBF3 films, the deposition rate of the YBF3 film layer is controlled to be 5±2%A / s.
8. The method for manufacturing a multi-band optical window according to claim 5, characterized in that: When evaporating the first to ninth ZnS films, the screen grid voltage of the RF ion source is controlled to be 1100±10%V, the screen grid current is 800±10%A, the accelerating electrode voltage is 700±10%V, the RF power is 430±10%KW, the argon gas flow rate is 100±10%sccm, and the oxygen gas flow rate is 60±10%sccm. The emitter voltage of the RF neutralizer is controlled to be 150±10%V, the emitter current is 2±10%A, the maintaining electrode voltage is 100±10%V, the maintaining electrode current is 1500±10%A, and the argon gas flow rate is 10±10%sccm.
9. The method for manufacturing a multi-band optical window according to claim 5, characterized in that: When evaporating the first to ninth ZnS films, the deposition rate of the ZnS film layer is controlled to be 3±2% A / s.
10. The method for manufacturing a multi-band optical window according to claim 5, characterized in that: The vacuum degree of the evaporation coating machine with RF ion source is controlled to 3.0*10 -5 torr-2.0*10 -5 torr, the temperature is controlled at 150±10%℃.
Citation Information
Patent Citations
High infrared transmission window with self cleaning hydrophilic surface
CN103323892A
Physical preparation method of film with visible light near-infrared anti-reflection function and special wetting function
CN104480434A
Visible light band-near infrared band-middle infrared band laser protection window and design method
CN107300782A
Double-sided coated glass applied to visible light and near-infrared light bands and production process of double-sided coated glass
CN109683214A
Multiband anti-reflection film system with zinc sulfide substrate and film coating method thereof
CN114035248A