Magneto-optic driven super-hydrophobic sponge and preparation method and application thereof
Through the magneto-optical-driven superhydrophobic sponge preparation method, the problems of flammable and insufficient self-cleaning performance of adsorbent materials are solved, and the effect of efficient absorption and separation of VOCs in water is achieved, and the rapid movement and evaporation rate is maintained under light drive, with excellent Self-cleaning and corrosion-proof properties.
Patent Information
- Application Number
- CN202411232548.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
AI Technical Summary
Existing adsorbent materials are flammable after adsorbing oil stains and lack self-cleaning properties, making it difficult to absorb volatile organic compounds (VOCs) pollutants in water for a long time and long-term, and there are safety risks in large areas of oil stain treatment.
The superhydrophobic sponge preparation method driven by magneto-optical drive is used to soak the dried sponge, magnetic treatment liquid and titanium nitride nanoparticles to form a sponge with magnetic, hydrophobic and photothermal characteristics, thereby improving its absorption efficiency and self-cleaning performance.
A low-cost and simple preparation process is realized. The sponge has high absorption efficiency, separation rate and separation range, and maintains a fast movement speed and evaporation rate under light drive. It has excellent self-cleaning performance and corrosion resistance, and is recycled. At the same time, the mass loss is small.
Smart Images

Figure CN119034696A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional materials, and in particular to a magneto-optically driven super-hydrophobic sponge and a preparation method and application thereof. Background Art
[0002] Volatile organic compounds (VOCs) are a common pollutant that is widely present in the atmosphere, soil and water. The World Health Organization (WHO) defines VOCs as a general term for volatile organic compounds with a melting point below room temperature and a boiling point between 50°C and 260°C. There are many sources of VOCs, among which the main causes of VOC emissions are human activities and natural production, such as solvents in paints and other coatings, adhesives in building wood, industrial activities, automobile exhaust emissions, biomass / biofuels, etc. Due to the wide range of VOC emission sources, it is inevitable that VOCs will be discharged into the water. VOCs in water bodies, including chloroform, benzene, toluene, 1,4-dichlorobenzene and 1,2-dichlorobenzene, are all known carcinogenic toxic substances, which will pose a great threat to human life and health. In addition, VOCs in water bodies are also harmful to other animals and plants. The presence of VOCs can change the ecological balance in the water body, inhibit the growth of phytoplankton and zooplankton, and lead to eutrophication and hypoxia in the water body.
[0003] In order to develop effective technologies for removing VOCs from water, many research projects are currently underway. These methods include multi-stage filtration, reverse osmosis, distillation and adsorption. Among them, the most commonly used is adsorption. The principle of adsorption is to use porous materials to absorb VOCs in the mixture of water and VOCs into the material. However, adsorption materials that have not been specially treated, such as porous carbon and sponges, will also absorb a large amount of water while absorbing oil, making it difficult to achieve the purpose of separating VOCs from water.
[0004] At present, the adsorbent material is made hydrophobic so that it can repel water while adsorbing pollutants. This can filter out the pollutants in the mixture, thereby achieving the purpose of separating VOCs from water. This type of hydrophobic material has received widespread attention due to its advantages such as high separation efficiency, low cost, recyclability, and no secondary pollution. Sponge is a green, environmentally friendly, low-cost material with a loose porous structure. After being hydrophobic, the material can efficiently and selectively absorb VOCs pollutants in water, and has broad prospects in the field of removing volatile pollutants from water. However, the recovery of sponge materials and the flammability of sponge materials after adsorbing oil pollution in large-scale oil pollution treatment are huge challenges. For example, a Chinese patent with publication number CN107602907A discloses a method for preparing a super-hydrophobic magnetic melamine resin sponge. The method firstly adopts a one-step solvent thermal method to synthesize hydrophobic magnetic ferroferric oxide particles, and then loads them on the surface of the melamine resin sponge under the action of an organic silicone adhesive. However, the modification process is complicated, the operation steps are cumbersome, and the flammability of the sponge material after adsorbing oil pollution is a huge safety hazard; and it does not have self-cleaning performance and cannot exert the performance of absorbing pollutants for a long time. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation method and application of a magneto-optically driven super-hydrophobic sponge, which has low preparation cost and simple preparation process. The obtained super-hydrophobic sponge has excellent magnetic, hydrophobic and photothermal properties, good self-cleaning performance and corrosion resistance, and has high absorption efficiency, separation rate and separation range for VOCs.
[0006] The embodiments of the present invention are implemented by the following technical solutions:
[0007] A method for preparing a magneto-optically driven super-hydrophobic sponge comprises the following steps:
[0008] (1) Sponge pretreatment: Take a dry sponge, soak it in an organic solvent, treat it with ultrasound, and then dry it to obtain the original sponge;
[0009] (2) Magnetic treatment liquid: Disperse the nano-magnetic particles and the low surface energy modifier in an organic solvent and stir to disperse them evenly to obtain the magnetic treatment liquid;
[0010] (3) Magnetic sponge: soaking the original sponge in the magnetic treatment solution obtained in step (2), ultrasonically treating the sponge, and then drying the sponge to obtain a magnetic sponge;
[0011] (4) Magneto-optical hydrophobic sponge: Titanium nitride nanoparticles are dispersed in an organic solvent, and then the magnetic sponge obtained in step (3) is added. After ultrasonic treatment, the sponge is dried to obtain the magneto-optically driven super-hydrophobic sponge.
[0012] Preferably, the sponge is any one of melamine sponge, polyurethane sponge, polyether sponge or melamine sponge.
[0013] Preferably, the ultrasonic treatment time is not less than 10 min.
[0014] Preferably, the organic solvent includes but is not limited to any one or more of anhydrous ethanol, ethyl acetate, butyl acetate, acetone, isopropanol, hexane or heptane; and the added amount is 50 ml.
[0015] Preferably, the sponge is dried by forced air drying, the drying temperature is 50-70° C., preferably 60° C., and the drying time is ≥ 2 h.
[0016] Preferably, the radius of the titanium nitride nanoparticles is 30-50 nm, preferably 40 nm.
[0017] Preferably, the low surface energy modifier is polydimethylsiloxane, and the polydimethylsiloxane comprises a polydimethylsiloxane precursor and a curing agent in a weight ratio of 10:1.
[0018] A magneto-optically driven super-hydrophobic sponge is prepared by the above preparation method.
[0019] Furthermore, the contact angle of the magneto-optically driven superhydrophobic sponge is ≥160°.
[0020] A magneto-optically driven super-hydrophobic sponge prepared by the above preparation method is used in VOCs water separation.
[0021] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:
[0022] 1. The present invention adopts an immersion method to load magnetic Fe3O4 nanoparticles and photothermal conversion material titanium nitride nanoparticles on a loose and porous sponge. This method has the advantages of simple process, convenient operation, strong controllability and low cost.
[0023] 2. The Fe3O4 nano-magnetic particles added in the present invention not only give the sponge magnetism, but also construct a micro-nano rough surface on the sponge skeleton, increasing the super-hydrophobicity of the sponge. Compared with the traditional super-hydrophobic sponge, the present invention can not only improve the absorption rate of VOCs on the water surface under magnetic drive, but also expand the working range of the sponge, and has excellent potential in water pollution treatment.
[0024] 3. The super-hydrophobic sponge prepared by the present invention has a highly loose porous structure inside, which ensures that the device has a high absorption efficiency for VOCs. In addition, relying on this structure, after the device absorbs saturated VOCs, it can also have a high evaporation rate of VOCs pollutants under light, and can maintain a faster movement speed under light drive.
[0025] 4. In addition to magnetic, hydrophobic and photothermal properties, the superhydrophobic sponge prepared by the present invention also has excellent self-cleaning performance, corrosion resistance and recyclability. After 10 cycles of absorption-evaporation, the device only loses 4% of its own mass, while its absorption capacity for VOCs remains basically unchanged. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 The scanning electron microscope images are of the original melamine sponge, the magnetic melamine sponge prepared in Comparative Example 1, and the magneto-optically driven superhydrophobic sponge prepared in Example 3;
[0028] Figure 2 The hydrophobic contact angle test results of the sponge samples obtained in Examples 1-3 of the present invention;
[0029] Figure 3 Schematic diagram of the original melamine sponge and the superhydrophobic sponge obtained in Example 3 absorbing VOCs pollutants under magnetic drive;
[0030] Figure 4 Schematic diagram of the movement speed of the superhydrophobic sponge obtained in Example 3 under light-driven irradiation with different laser powers. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0032] The following is a detailed description of a magneto-optically driven super-hydrophobic sponge and its preparation method and application provided in an embodiment of the present invention.
[0033] A method for preparing a magneto-optically driven super-hydrophobic sponge comprises the following steps:
[0034] (1) Sponge pretreatment: Take a dry sponge, soak it in an organic solvent, treat it with ultrasound, and then dry it to obtain the original sponge;
[0035] The sponge can be any one of melamine sponge, polyurethane sponge, polyether sponge or melamine sponge. Preferably, melamine sponge is used, and the cutting size is 2 cm×2 cm×1 cm. The sponge is dried by forced air drying, and the drying temperature is 50-70°C, preferably 60°C, and the drying time is ≥2h. The loose porous structure of melamine sponge can absorb more VOCs, and more importantly, it can be used as an excellent loading medium. The surface of the sponge is cleaned by pretreatment to prevent pollutants from clogging the sponge pores and affecting the subsequent modification and adsorption performance of the sponge.
[0036] (2) Magnetic treatment liquid: Disperse the nano-magnetic particles and the low surface energy modifier in an organic solvent and stir to disperse them evenly to obtain the magnetic treatment liquid;
[0037] Among them, the nano magnetic particles can be selected from Fe2O3 and Fe3O4 nano particles, preferably Fe3O4 nano particles, and the low surface energy modifier is polydimethylsiloxane, specifically, a polydimethylsiloxane precursor and a curing agent are included in a weight ratio of 10:1; through the treatment of this step, the nano magnetic particles and the low surface energy modifier are organically combined to form an excellent magnetic treatment liquid, which is convenient for subsequent loading between the sponge;
[0038] (3) Magnetic sponge: soaking the original sponge in the magnetic treatment solution obtained in step (2), ultrasonically treating the sponge, and then drying the sponge to obtain a magnetic sponge;
[0039] Thus, the nano-magnetic particles are loaded on the loose and porous sponge collectively through a low surface energy modifier, and the load is stabilized, so that the sponge has magnetism, and a rough surface of micro-nano level is constructed on the sponge skeleton, which increases the super-hydrophobicity of the sponge, and then the VOCs in the VOCs-containing wastewater can be efficiently absorbed. Compared with the traditional super-hydrophobic sponge, the present invention can not only improve the absorption rate of VOCs on the water surface under magnetic drive, but also expand the working range of sponge absorption, and has excellent potential in water pollution treatment;
[0040] (4) Magneto-optical hydrophobic sponge: Titanium nitride nanoparticles are dispersed in an organic solvent, and then the magnetic sponge obtained in step (3) is added. After ultrasonic treatment, the sponge is dried to obtain the magneto-optically driven super-hydrophobic sponge. The radius of the titanium nitride nanoparticles is 30-50 nm, preferably 40 nm. The sponge obtained in this way has improved photothermal performance. After the sponge absorbs saturated VOCs, it can still have a high evaporation rate of VOCs pollutants under light and can maintain a faster movement speed under light drive.
[0041] More specifically: After adding the low surface energy modifier, the surface of the sponge is coated with PDMS, and the liquid is blocked by the PDMS on the surface of the sponge and cannot completely penetrate the surface of the material, so that the sponge has hydrophobicity. In addition, the added nano magnetic particles give the melamine sponge magnetism, and the titanium nitride nanoparticles give the sponge photothermal properties. The two also simultaneously construct a micro-nano level rough surface on the melamine sponge skeleton. According to the Cassier-Baxter theory, the rough hierarchical structure of the sponge surface increases, and the formed pores capture a large amount of air, so that the contact area between the solid and the liquid is reduced, and the water droplets cannot fill the pores on the sponge surface but are suspended on the sponge surface, thereby increasing the super hydrophobicity of the sponge. Therefore, under the joint action of the low surface energy modifier, the nano magnetic particles and the melamine sponge, the sponge is prompted to achieve a typical Cassier-Baxter super hydrophobic state.
[0042] After adding photothermal materials to the sponge, when the sponge absorbs VOCs to saturation, the sponge can heat up under sunlight to volatilize the VOCs, making the sponge reusable. In addition, when the laser irradiates its surface, the surface of the sponge will heat up rapidly, and the temperature is transferred from the sponge to the water surface. The temperature on both sides of the sponge is different. Due to the Marangoni effect, the tension on both sides of the sponge is different, so that the sponge can move on the water surface under light drive. This water surface drive can be used in many aspects, such as water surface transportation, mobile obstacle avoidance, water surface oil stain cleaning and drug delivery.
[0043] More importantly, the sponge prepared by the preparation method of the present invention has excellent self-cleaning performance and anti-corrosion ability in addition to magnetic, hydrophobic and photothermal properties.
[0044] During use, the inventors found that: because the dust on the surface of the sponge during use will hinder the light absorption of the material and reduce the hydrophobicity of the material, it is not conducive to the application of the material. After loading nano magnetic particles and melamine sponge on the sponge surface, a super hydrophobic photothermal sponge is formed. When dust falls on the sponge surface, due to the rolling motion of water droplets, pollutants are easily taken away by water balls, and a clean surface is left, so that the surface can be kept clean, which is conducive to the anti-fouling and dustproof of the material and can extend the service life of the material. In addition, the material also has good corrosion resistance. During the application process, if the solution of strong acid or strong alkali in the wastewater may corrode the sponge material, the surface is damaged, thereby reducing the functional characteristics of the material. After the sponge surface is coated with low surface energy modifier, nano magnetic particles and melamine sponge, it has good super hydrophobicity, and the solution of strong acid or strong alkali in the application environment is blocked by the super hydrophobic layer on the surface of the material and cannot penetrate the inside of the material, thereby protecting the surface of the material and the rough surface structure of the micro-nano level, which is conducive to improving the application performance of the sponge material in a corrosive environment.
[0045] Preferably, the ultrasonic treatment time is not less than 10 min.
[0046] Preferably, the above-mentioned organic solvent includes, but is not limited to, any one or more of anhydrous ethanol, ethyl acetate, butyl acetate, acetone, isopropanol, hexane or heptane.
[0047] A magneto-optically driven super-hydrophobic sponge is prepared by the above preparation method, and the contact angle of the obtained magneto-optically driven super-hydrophobic sponge is ≥160°.
[0048] A magneto-optically driven super-hydrophobic sponge prepared by the above preparation method is used in VOCs water separation.
[0049] Example 1
[0050] This embodiment provides a method for preparing a magneto-optically driven super-hydrophobic sponge, comprising the following steps:
[0051] (1) Cut the melamine sponge into a shape of 2 cm × 2 cm × 1 cm, soak it in 50 ml of anhydrous ethanol, and treat it with ultrasound for 10 min. After the ultrasound treatment, dry it in an electric hot air drying oven at 60 °C for 2 h.
[0052] (2) Disperse 1.5 g of Fe3O4 nanoparticles, 0.9 g of PDMS precursor and 0.09 g of PDMS curing agent in 50 mL of ethyl acetate organic phase and stir to make them evenly dispersed;
[0053] (3) Using tweezers, slowly immerse the dry and clean melamine sponge obtained in step (1) in the organic phase obtained in step (2). The melamine sponge will sink to the bottom of the liquid. Ultrasonic treatment is performed for 20 min. After immersion, the sponge is dried in an electric blast drying oven at 60° C. for 2 h to obtain a magnetic melamine sponge.
[0054] (4) Disperse 1.5 g of titanium nitride nanoparticles in 50 mL of ethyl acetate organic phase and stir to make it evenly dispersed;
[0055] (5) Slowly immerse the magnetic melamine sponge in step (3) in the organic phase obtained in step (4) and treat it with ultrasound for 20 min. After the ultrasound is completed, dry it in an electric heated blast drying oven at 60°C for 2 h to obtain the final magneto-optically driven superhydrophobic sponge.
[0056] Example 2
[0057] This embodiment provides a method for preparing a magneto-optically driven super-hydrophobic sponge, comprising the following steps:
[0058] (1) Cut the melamine sponge into a shape of 2 cm × 2 cm × 1 cm, soak it in 50 ml of anhydrous ethanol, and treat it with ultrasound for 20 min. After the ultrasound treatment, dry it in an electric hot air drying oven at 65 °C for 2 h.
[0059] (2) Disperse 1.50 g of Fe3O4 nanoparticles, 1.2 g of PDMS precursor and 0.12 g of PDMS curing agent in 50 mL of ethyl acetate organic phase and stir to make them evenly dispersed;
[0060] (3) Using tweezers, slowly immerse the dry and clean melamine sponge obtained in step (1) in the organic phase obtained in step (2). The melamine sponge will sink to the bottom of the liquid. Ultrasonic treatment is performed for 30 min. After immersion, the sponge is dried in an electric blast drying oven at 65°C for 2 h to obtain a magnetic melamine sponge.
[0061] (4) Disperse 1.5 g of titanium nitride nanoparticles in 50 mL of ethyl acetate organic phase and stir to ensure uniform dispersion;
[0062] (5) Slowly immerse the magnetic melamine sponge in step (3) in the organic phase obtained in step (4) and treat it with ultrasound for 20 min. After the ultrasound is completed, dry it in an electric heated air drying oven at 65°C for 2 h to obtain the final magneto-optically driven superhydrophobic sponge.
[0063] Example 3
[0064] This embodiment provides a method for preparing a magneto-optically driven super-hydrophobic sponge, comprising the following steps:
[0065] (1) Cut the melamine sponge into a shape of 2 cm × 2 cm × 1 cm, soak it in 50 ml of anhydrous ethanol, and treat it with ultrasound for 30 min. After the ultrasound treatment, dry it in an electric hot air drying oven at 70 °C for 2 h.
[0066] (2) Disperse 1.50 g of Fe3O4 nanoparticles, 1.50 g of PDMS precursor and 0.15 g of PDMS curing agent in 50 mL of ethyl acetate organic phase and stir to make them evenly dispersed;
[0067] (3) Using tweezers, slowly immerse the dry and clean melamine sponge obtained in step (1) in the organic phase obtained in step (2). The melamine sponge will sink to the bottom of the liquid. Ultrasonic treatment is performed for 25 min. After immersion, the sponge is dried in an electric blast drying oven at 70° C. for 2 h to obtain a magnetic melamine sponge.
[0068] (4) Disperse 1.50 g of titanium nitride nanoparticles in 50 mL of ethyl acetate organic phase and stir to ensure uniform dispersion;
[0069] (5) The magnetic melamine sponge in step (3) is slowly immersed in the organic phase in step (4) and treated with ultrasound for 25 min. After the ultrasound is completed, it is dried in an electric heated air drying oven at 70°C for 2 h to obtain the final magneto-optically driven superhydrophobic sponge.
[0070] Comparative Example 1
[0071] The difference between this comparative example and Example 3 is that it does not contain steps (4) to (5); that is, the magnetic melamine sponge obtained in this comparative example is obtained.
[0072] Experimental Example 1
[0073] The original melamine sponge, the magnetic melamine sponge prepared in Comparative Example 1, and the magneto-optically driven super-hydrophobic sponge prepared in Example 3 were used as experimental groups 1-3. The microstructures of the samples of experimental groups 1-3 were analyzed, and the scanning electron microscope images thereof are shown in FIG. Figure 1 ,in Figure 1 (a)-(c) are the microscopic morphologies of the original melamine sponge, the magnetic melamine sponge prepared in Comparative Example 1, and the magneto-optically driven superhydrophobic sponge prepared in Example 3, respectively. The left side of each figure is an image of lower magnification, and the right side is an image of higher magnification.
[0074] Depend on Figure 1From the lower magnification images, we can see that each sponge sample is loose and porous in microscopic view, with the diameter of each pore being on the order of 100 μm, while the diameter of the sponge skeleton is only on the order of 10 μm. The loose and porous structure determines the good absorption capacity of the sponge for liquid.
[0075] Further, by Figure 1 (b), (c) and Figure 1 (a) From the comparison of the right sides of the figures, it can be seen that the skeleton in (a) is basically smooth, with only a few impurities or defects, which may be caused during the production process; Figure 1 The skeletons in (b) and (c) are bonded with a large amount of rough materials, which indicates that Fe3O4 nanoparticles and titanium nitride nanoparticles are deposited on the melamine sponge skeleton, forming a rough surface morphology at the micro-nano scale, which increases the superhydrophobicity of the sponge to a certain extent.
[0076] Experimental Example 2
[0077] The hydrophobic contact angle of the sponge samples obtained by adding different proportions of low surface energy modifier PDMS precursor and photothermal material titanium nitride nanoparticles in Examples 1-3 was tested. The test results are shown in Figure 2 ,Depend on Figure 2 The results show that when the addition ratio of PDMS and titanium nitride nanoparticles in Example 3 is 1:1, the contact angle of the sample reaches the maximum, reaching 163°, and the samples used in the subsequent VOCs and water separation experiments and light-driven experiments are all at this concentration.
[0078] Experimental Example 3
[0079] The original melamine sponge and the super-hydrophobic sponge obtained in Example 3 were tested for absorbing VOCs pollutants under magnetic drive. The schematic diagram of the absorption process is shown in Figure 3 ;in Figure 3 (a) is a schematic diagram of the absorption process of the original melamine sponge; Figure 3 (b) is a schematic diagram of the absorption process of the superhydrophobic sponge obtained in Example 3;
[0080] in, Figure 3 (a) Under magnetic drive, the original sponge quickly absorbs water after contacting the water body due to its lack of superhydrophobicity, and then sinks into the water body in a short time (within 10 s). It remains stationary in the subsequent experimental process, and its absorption effect on VOCs pollutants is very limited. Figure 3In (b), tweezers are used to manipulate the NdFeB permanent magnet to magnetically drive the sponge floating on the surface of the water, so that the superhydrophobic sponge actively moves on the surface of the water under magnetic drive, accelerating the surface liquid flow and the absorption of VOCs pollutants by the sponge. Most of the VOCs pollutants are absorbed within 50 seconds, and almost all of the VOCs pollutants are absorbed within 75 seconds, completing the cleaning of the water. Magnetic drive increases the absorption rate of VOCs pollutants by the superhydrophobic sponge, and also expands the absorption range of VOCs pollutants, which can purify a wide area of water surface.
[0081] Experimental Example 4
[0082] Under laser irradiation, the relationship between the speed of the super-hydrophobic sponge obtained in Example 3 on the water surface and the irradiated laser power was tested, and the results are shown in Figure 4 ,Depend on Figure 4 The results show that the movement speed increases with the increase of laser power. When the laser power is 2.5w / cm -2 The movement speed is 15.93mm / s. This water surface drive can be used in many aspects, such as water surface transportation, mobile obstacle avoidance, water surface oil stain cleaning, drug delivery, etc.
[0083] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a magneto-optically driven super-hydrophobic sponge, characterized in that: The following steps are involved: (1) Sponge pretreatment: Take a dry sponge, soak it in an organic solvent, treat it with ultrasound, and then dry it to obtain the original sponge; (2) Magnetic treatment liquid: Disperse the nano-magnetic particles and the low surface energy modifier in an organic solvent and stir to disperse them evenly to obtain the magnetic treatment liquid; (3) Magnetic sponge: soaking the original sponge in the magnetic treatment solution obtained in step (2), ultrasonically treating the sponge, and then drying the sponge to obtain a magnetic sponge; (4) Magneto-optical hydrophobic sponge: Titanium nitride nanoparticles are dispersed in an organic solvent, and then the magnetic sponge obtained in step (3) is added. After ultrasonic treatment, the sponge is dried to obtain the magneto-optically driven super-hydrophobic sponge.
2. The method for preparing a magneto-optically driven super-hydrophobic sponge according to claim 1, wherein The mass ratio of the nano magnetic particles to the low surface energy modifier is 1-2:1; the mass ratio of the low surface energy modifier to the titanium nitride nano particles is 0.4-1:
1.
3. The preparation method of the magneto-optically driven super-hydrophobic sponge according to claim 1, wherein The sponge is any one of melamine sponge, polyurethane sponge, polyether sponge or melamine sponge.
4. The method for preparing a magneto-optically driven super-hydrophobic sponge according to claim 1, wherein The ultrasonic treatment time is not less than 10 min.
5. The method for preparing a magneto-optically driven super-hydrophobic sponge according to claim 1, wherein The organic solvent is any one or more of anhydrous ethanol, ethyl acetate, butyl acetate, acetone, isopropanol, hexane or heptane.
6. The preparation method of the magneto-optically driven super-hydrophobic sponge according to claim 1, characterized in that, The sponge is dried by forced air drying at a temperature of 50-70°C for a drying time of ≥2h.
7. The method for preparing a magneto-optically driven super-hydrophobic sponge according to claim 1, wherein: The low surface energy modifier is polydimethylsiloxane, and the polydimethylsiloxane comprises a polydimethylsiloxane precursor and a curing agent in a weight ratio of 10:
1.
8. A magneto-optically driven super-hydrophobic sponge, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.
9. The magneto-optically driven super-hydrophobic sponge according to claim 8, characterized in that: The contact angle of the magneto-optically driven super-hydrophobic sponge is ≥160°.
10. Use of a magneto-optically driven super-hydrophobic sponge prepared by the preparation method according to any one of claims 1 to 7 in treating wastewater containing VOCs.
Citation Information
Patent Citations
Preparation method of super-hydrophobic magnetic melamine resin sponge
CN107602907A