Positive electrode material of ultra-high power pulse type energy storage device and preparation method of positive electrode material

Through transition metal lithium oxide positive electrode material and electrostatic spraying technology mixed with nano- and micro-sized particle sizes, the shortcomings of existing energy storage devices in high-power pulse power applications are solved, and high energy density and high-magnification pulse cycles are achieved Capable energy storage devices, suitable for new energy vehicles and aerospace power supplies.

CN119050327AActive Publication Date: 2024-11-29GUIZHOU MEILING POWER SUPPLY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411344123.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-29
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

In high-power pulse power applications, existing energy storage devices are difficult to meet the needs of high-power pulse power supplies in new energy vehicles and other fields, and their cycle life is insufficient.

Method used

Using transition metal lithium oxide positive electrode material mixed with nano-scale and micro-scale particle size, an energy storage device with high-magnification pulse and cycle capability is prepared through a high-energy ball mill evenly mixing and combined with electrostatic spraying technology.

Benefits of technology

On the premise of ensuring a certain energy density, the high-power pulse performance of energy storage devices is significantly improved, suitable for new energy vehicles and aerospace power supply, and improves pulse discharge performance and cycling capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050327A_ABST
    Figure CN119050327A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an ultra-high power pulse type energy storage device positive electrode material in the technical field of novel energy storage devices, and the preparation method comprises the following steps: S1, putting transition metal lithium-intercalated oxides with micron-scale and nano-scale particle sizes into a high-energy ball mill according to a mass ratio of (70-95): (5-30), and adding a proper amount of a solvent to make the mixture form slurry; the high-energy ball mill carries out ball milling for 2-6 h at the rotating speed of 200-400 r / min, and a mixed positive electrode material And S2, fully and uniformly stirring the prepared mixed positive electrode material, a conductive agent and a binder, then adding an organic solvent, uniformly stirring again to prepare spraying slurry, uniformly spraying the slurry on the surface of a base material through electrostatic spraying, and drying to obtain the electrostatic spraying method mixed material positive electrode material. The capacitive energy storage property of the nanoscale positive electrode material and the battery energy storage property of the micron-sized positive electrode material are utilized, so that the high-power pulse performance of an energy storage device is greatly improved on the premise of ensuring that the battery has certain energy density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of novel energy storage devices, and in particular to a positive electrode material of an ultra-high power pulse type energy storage device and a preparation method thereof. Background Art

[0002] In recent years, with the advancement of battery technology and manufacturing processes, the performance indicators of secondary energy storage batteries such as lithium-ion batteries have been continuously improved, and their applications in various fields have become more and more extensive. From new energy power batteries to special equipment such as aerospace, such application scenarios have higher requirements for the power, energy density and cycle life of pulse power supplies. Therefore, it is necessary and urgent to prepare energy storage devices with excellent performance and high-power pulse discharge.

[0003] The present application prepares a lithium cobalt oxide positive electrode material with a mixture of nano-scale and micron-scale particles, and uses a commercial hard carbon material as a negative electrode material to prepare an energy storage device with excellent high-rate pulse and high-rate cycle performance. At the same time, it has a certain energy density, which can meet the needs of new energy vehicles and other fields for high-power pulse power supplies. Summary of the invention

[0004] The present invention aims to provide an ultra-high power pulse energy storage device and a preparation method thereof, which utilizes the capacitive energy storage properties of nano-scale positive electrode materials and the battery energy storage properties of micron-scale positive electrode materials to greatly improve the high-power pulse performance of the energy storage device (1s pulse rate ≥100C) while ensuring that the battery has a certain energy density (>80Wh / kg).

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a positive electrode material for an ultra-high power pulse type energy storage device comprises the following steps:

[0007] S1. Place transition metal lithium intercalation oxides of micron-scale and nanometer-scale particle sizes in a high-energy ball mill at a mass ratio of 70-95:5-30, and add an appropriate amount of solvent to form a slurry; the high-energy ball mill is milled at a speed of 200-400 r / min for 2-6 hours to obtain a mixed positive electrode material of transition metal lithium intercalation oxides with a mixture of micron-scale and nanometer-scale particle sizes;

[0008] S2. After fully stirring the prepared mixed positive electrode material, conductive agent and binder, add an organic solvent, stir again to make a spray slurry, spray the slurry evenly on the surface of the substrate by electrostatic spraying, and obtain the electrostatic spraying mixed material positive electrode material after drying.

[0009] Working principle and beneficial effects of the present invention:

[0010] By uniformly mixing nano- and micron-sized particles of transition metal embedded lithium oxide, and utilizing the capacitance properties of nano-sized particles and the battery properties of micron-sized particles, the pulse discharge performance of the energy storage device can be greatly improved while having a high energy density, thereby preparing a new type of ultra-high power pulse energy storage device suitable for new energy vehicle power batteries, aerospace power supply and other fields.

[0011] Since the particle size of transition metal lithium-embedded oxides at the micron and nanometer levels is small, when conventional mixing methods are used, such as planetary mixers or ultrasonic dispersion, the densities of the two particle sizes of materials are different. Dispersion using the above two methods may cause stratification, resulting in uneven mixing. However, the present application uses small-diameter balls, medium-diameter balls, and large-diameter balls for low-speed, short-time ball milling mixing, which will not cause stratification, and the mixing is more uniform, making the spraying on the substrate surface more uniform, thereby improving the high-rate pulse and high-rate cycle capabilities of the positive electrode material.

[0012] Optimized, the transition metal lithium-embedded oxide includes LiCoO2, LiMn2O4, LiFePO4, LiNi 1~x~ y Co y Mn x O2 (NCM ternary material), LiNi 1~x~y Co y Al x O2 (NCA ternary material), LiM x Mn 2~x O4 (M is Fe or Co doped atoms) is a positive electrode material for lithium-ion batteries.

[0013] Optimally, the mass proportion of nano-sized particles in the mixture is 5-30%.

[0014] Optimally, the mass ratio of the stainless steel balls to the milled material in the high-energy ball mill is 3 to 5:1.

[0015] Optimally, the mass ratio of the small diameter ball, the medium diameter ball and the large diameter ball in the stainless steel ball is 4-5:3-4:2, and the diameters of the large ball, the medium ball and the small ball are 20 mm, 10 mm and 5 mm respectively.

[0016] Optimized, S1 placed the mixed cathode material obtained by ball milling in a vacuum oven and dried it at a temperature of 60°C to 80°C for 12 to 24 hours.

[0017] Optimally, during the S2 electrostatic spraying, the single-side spraying of the substrate surface is dried after completion, and the other side of the substrate surface is treated in the same way.

[0018] Optimally, the conductive agent is CNTs and SP, the binder is PVDF, the added mass ratio of the mixed positive electrode material and CNTs, SP, and PVDF is: 85-92.5:2.5-5:2.5-5:2.5-5; and the organic solvent is N-methylpyrrolidone.

[0019] Optimized, the spray slurry is injected into the spray gun of the electrostatic spraying equipment, the spraying distance is adjusted to 5-20 cm, the spraying speed is 1 cm / s-3 cm / s, the electrostatic spraying voltage is set to 10-20 kV, the ambient temperature is 25°C, the spray slurry is evenly sprayed on the surface of the substrate, and the spraying thickness is 15-35 μm.

[0020] A positive electrode material obtained by a method for preparing a positive electrode material for an ultra-high power pulse type energy storage device. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM photo of the pole piece of Example 1 of the present invention;

[0022] Figure 2 This is a SEM photo of the pole piece of Example 2 of the present invention;

[0023] Figure 3 for Figure 3 SEM photo of the pole piece of comparative example 1 of the present invention;

[0024] Figure 4 This is a SEM photo of the pole piece of comparative example 2 of the present invention;

[0025] Figure 5 1C discharge curves of the battery assembled with the pole pieces of Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 of the present invention;

[0026] Figure 6 100C pulse discharge curves of the battery assembled with the pole pieces of Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 of the present invention;

[0027] Figure 7 500C pulse discharge curves of the battery assembled with the pole pieces of Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 of the present invention;

[0028] Figure 8 10C charge / 20C discharge cycle curves of the battery assembled with the electrode sheets of Example 1 and Example 2 of the present invention and Comparative Examples 1, 2, 3, 4 and 5. DETAILED DESCRIPTION

[0029] The following is further described in detail through specific implementation methods:

[0030] Example 1

[0031] (1) Preparation of nanoparticle lithium cobalt oxide positive electrode materials

[0032] Weigh 10g of lithium cobalt oxide material with a particle size of 100nm and 90g of particle size D 50 =5μm lithium cobalt oxide (LiCoO2) material is placed in a ball mill with stainless steel balls, wherein the mass ratio of the stainless steel balls to the ball-milled material is 3:1, and the mass ratio of the small diameter balls, medium diameter balls, and large diameter balls in the stainless steel balls is 4:4:2.

[0033] An appropriate amount of anhydrous ethanol is added to the ball mill to form a proper slurry. The ball mill is then placed in a high-energy ball mill and milled at a speed of 400 r / min for 4 hours. The milled material is placed in a vacuum oven and dried at 80°C for 24 hours to remove the residual solvent, thereby obtaining a lithium cobalt oxide mixed positive electrode material with a mixture of nano-scale and micro-scale particle sizes.

[0034] (2) Preparation of electrostatically sprayed nanoparticle lithium cobalt oxide positive electrode

[0035] The prepared nano-particle lithium cobalt oxide mixed positive electrode material and conductive agent (CNTs, SP) and binder (PVDF) are placed in a stirring tank with a mass ratio of 92.5:2.5:2.5:2.5. After being fully stirred, the organic solvent N-methylpyrrolidone (NMP) is added. The added mass ratio of active material to NMP is 1:1.3. After stirring evenly, a spray slurry is prepared.

[0036] Inject the spray slurry into the spray gun of the electrostatic spray equipment, adjust the spray distance to 10 cm, the spray speed to 2 cm / s, set the electrostatic spray voltage to 12 kV, the ambient temperature to 25 ° C, and spray the slurry evenly on the surface of the aluminum foil with a spray thickness of 20 μm.

[0037] After one side is sprayed, it is placed in an oven at 80°C for drying, and then the other side is sprayed with the same parameters. After drying, the electrostatically sprayed nano-particle lithium cobalt oxide positive electrode is obtained. The SEM photo of the coated electrode is shown in the figure. Figure 1 shown.

[0038] Example 2

[0039] (1) Nanoparticle LiN 0.5 Co 0.2 Mn 0.3 Preparation of O2 cathode materials

[0040] Weigh 30g of LiN with a particle size of 100nm 0.5 Co 0.2 Mn 0.3 O2 material, 70g particle size D50 =2μm LiN 0.5 Co 0.2 Mn 0.3 The O2 material is placed in a ball mill with stainless steel balls, wherein the mass ratio of the stainless steel balls to the ball-milled material is 4:1, and the mass ratio of the small-diameter balls, medium-diameter balls, and large-diameter balls among the stainless steel balls is 5:3:2.

[0041] Add an appropriate amount of water or anhydrous ethanol to the ball mill to form a proper slurry. Then place the ball mill in a high-energy ball mill and mill at a speed of 400 r / min for 4 hours. Place the milled material in a vacuum oven and dry it at 80°C for 24 hours to remove the residual solvent, and obtain a lithium cobalt oxide mixed positive electrode material with a mixture of nano-sized and micron-sized particles.

[0042] (2) Preparation of electrostatically sprayed nanoparticle lithium cobalt oxide positive electrode

[0043] The prepared nano-particle lithium cobalt oxide mixed positive electrode material and conductive agent (CNTs, SP), binder (PVDF) are placed in a stirring tank with a mass ratio of 90:3:3:4. After being fully stirred, the organic solvent N-methylpyrrolidone (NMP) is added. The added mass ratio of active material to NMP is 1:1.4. After stirring evenly, a spray slurry is prepared.

[0044] Inject the spray slurry into the spray gun of the electrostatic spray equipment, adjust the spray distance to 10 cm, the spray speed to 2 cm / s, set the electrostatic spray voltage to 12 kV, the ambient temperature to 25 ° C, and spray the slurry evenly on the surface of the aluminum foil with a spray thickness of 20 μm.

[0045] After one side is sprayed, it is placed in an oven at 80°C for drying, and then the other side is sprayed with the same parameters. After drying, the electrostatically sprayed nano-particle lithium cobalt oxide positive electrode is obtained. The SEM photo of the coated electrode is shown in the figure. Figure 2 shown.

[0046] Comparative Example 1

[0047] Micron-sized particles of lithium cobalt oxide (particle size D 50 =7μm) positive electrode material and conductive agent (CNTs, SP), binder (PVDF) are placed in a stirring tank with a mass ratio of 92.5:2.5:2.5:2.5. After fully stirring, the organic solvent N-methylpyrrolidone (NMP) is added. The mass ratio of active material to NMP is 1:1.2. After stirring, a spray slurry is prepared.

[0048] Inject the spray slurry into the spray gun of the electrostatic spray equipment, adjust the spray distance to 10 cm, the spray speed to 2 cm / s, set the electrostatic spray voltage to 12 kV, the ambient temperature to 25 ° C, and spray the slurry evenly on the surface of the aluminum foil with a spray thickness of 20 μm.

[0049] After one side is sprayed, it is placed in an oven at 80°C for drying, and then the other side is sprayed with the same parameters. After drying, the electrostatically sprayed nano-particle lithium cobalt oxide positive electrode is obtained. The SEM photo of the coated electrode is shown in the figure. Figure 3 shown.

[0050] Comparative Example 2

[0051] (1) Nanoparticle LiN 0.8 Co 0.1 Mn 0.1 Preparation of O2 cathode materials

[0052] Weigh 55g of LiN with a particle size of 100nm 0.8 Co 0.8 Mn 0.1 O2 material, 45g LiN with a particle size of 7 microns 0.8 Co 0.8 Mn 0.1 The O2 material is placed in a ball mill with stainless steel balls, wherein the mass ratio of the stainless steel balls to the ball-milled material is 3:1, and the mass ratio of the small-diameter balls, medium-diameter balls, and large-diameter balls among the stainless steel balls is 4:4:2.

[0053] Add an appropriate amount of water or anhydrous ethanol to the ball mill to form a suitable slurry. Then place the ball mill in a high-energy ball mill and mill at a speed of 500r / min for 3h. Place the milled material in a vacuum oven and dry it at 80°C for 12-24h to remove the residual solvent to obtain LiN mixed with nano-sized and micron-sized particles. 0.8 Co 0.1 Mn 0.1 O2 mixed positive electrode material.

[0054] (2) Electrostatic spraying of nanoparticles LiN 0.8 Co 0.1 Mn 0.1 Preparation of O2 positive electrode

[0055] The prepared nanoparticles LiN 0.8 Co 0.1 Mn 0.1O2 mixed positive electrode material and conductive agent (CNTs, SP), binder (PVDF) are placed in a stirring tank with a mass ratio of 85:5:5:5. After fully stirring, the organic solvent N-methylpyrrolidone (NMP) is added. The added mass ratio of active material to NMP is 1:1.5. After stirring evenly, a spray slurry is prepared.

[0056] Inject the spray slurry into the spray gun of the electrostatic spray equipment, adjust the spray distance to 10 cm, the spray speed to 2 cm / s, set the electrostatic spray voltage to 12 kV, the ambient temperature to 25 ° C, and spray the slurry evenly on the surface of the aluminum foil with a spray thickness of 20 μm.

[0057] After one side is sprayed, it is placed in an oven at 80°C for drying, and then the other side is sprayed with the same parameters. After drying, the electrostatically sprayed nano-particle lithium cobalt oxide positive electrode is obtained. The SEM photo of the coated electrode is shown in the figure. Figure 4 shown.

[0058] In the above Example 1, Example 2 and Comparative Example 2, the diameters of the large ball, the medium ball and the small ball are 20 mm, 10 mm and 5 mm respectively.

[0059] Comparative Example 3: Eliminating the ball milling step based on Example 1

[0060] Weigh 10g of lithium cobalt oxide material with a particle size of 100nm and 90g of particle size D 50 =5μm lithium cobalt oxide (LiCoO2) material is used as the positive electrode active material. The positive electrode active material, conductive agent (CNTs, SP), and binder (PVDF) are placed in a stirring tank at a mass ratio of 92.5:2.5:2.5:2.5, and the organic solvent N-methylpyrrolidone (NMP) is added after being fully stirred. The mass ratio of active material to NMP is 1:1.3, and the spray slurry is prepared after being stirred evenly.

[0061] Inject the spray slurry into the spray gun of the electrostatic spray equipment, adjust the spray distance to 10 cm, the spray speed to 2 cm / s, set the electrostatic spray voltage to 12 kV, the ambient temperature to 25 ° C, and spray the slurry evenly on the surface of the aluminum foil with a spray thickness of 20 μm.

[0062] After the single-side spraying is completed, it is placed in an oven to dry at 80°C, and then the other side is sprayed according to the same parameters. After drying, the electrostatically sprayed nano-particle lithium cobalt oxide positive electrode is obtained.

[0063] Comparative Example 4 uses other methods to mix on the basis of Example 1

[0064] (1) Preparation of nanoparticle lithium cobalt oxide positive electrode materials

[0065] Weigh 10g of lithium cobalt oxide material with a particle size of 100nm and 90g of particle size D 50 =5μm lithium cobalt oxide (LiCoO2) material is placed in a planetary mixer and stirred at a speed of 90r / min for 2h to obtain nano-particle lithium cobalt oxide mixed positive electrode material.

[0066] (2) Preparation of electrostatically sprayed nanoparticle lithium cobalt oxide positive electrode

[0067] The prepared nano-particle lithium cobalt oxide mixed positive electrode material and conductive agent (CNTs, SP) and binder (PVDF) are placed in a stirring tank with a mass ratio of 92.5:2.5:2.5:2.5. After being fully stirred, the organic solvent N-methylpyrrolidone (NMP) is added. The added mass ratio of active material to NMP is 1:1.3. After stirring evenly, a spray slurry is prepared.

[0068] Inject the spray slurry into the spray gun of the electrostatic spray equipment, adjust the spray distance to 10 cm, the spray speed to 2 cm / s, set the electrostatic spray voltage to 12 kV, the ambient temperature to 25 ° C, and spray the slurry evenly on the surface of the aluminum foil with a spray thickness of 20 μm.

[0069] After the single-side spraying is completed, it is placed in an oven to dry at 80°C, and then the other side is sprayed according to the same parameters. After drying, the electrostatically sprayed nano-particle lithium cobalt oxide positive electrode is obtained.

[0070] Comparative Example 5: Based on Example 1, the addition of micron-sized lithium cobalt oxide is eliminated.

[0071] Weigh 100g of lithium cobalt oxide material with a particle size of 100nm as the positive electrode active material. Put the positive electrode active material, conductive agent (CNTs, SP), and binder (PVDF) in a stirring tank at a mass ratio of 92.5:2.5:2.5:2.5, stir well, add organic solvent N-methylpyrrolidone (NMP), and add the mass ratio of active material to NMP at 1:1.3, stir well to make a spray slurry.

[0072] Inject the spray slurry into the spray gun of the electrostatic spray equipment, adjust the spray distance to 10 cm, the spray speed to 2 cm / s, set the electrostatic spray voltage to 12 kV, the ambient temperature to 25 ° C, and spray the slurry evenly on the surface of the aluminum foil with a spray thickness of 20 μm.

[0073] After the single-side spraying is completed, it is placed in an oven to dry at 80°C, and then the other side is sprayed according to the same parameters. After drying, the electrostatically sprayed nano-particle lithium cobalt oxide positive electrode is obtained.

[0074] Preparation method of negative electrode: weigh 2.5g superconducting carbon black, 2.5g carbon nanotubes, 5.0g polyvinylidene fluoride (PVDF), and 90g commercial hard carbon material and add them into a blender, stir at a stirring speed of 30-90r / min for 1-2h until the powder is evenly mixed. Add NMP into the blender in 4 times, stir for 1-1.5h each time NMP is added, and the coating process is performed to prepare a hard carbon negative electrode.

[0075] The specific implementation process is as follows: Use the positive electrode sheets prepared in Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, and Comparative Example 5 to assemble soft-pack batteries. The specific process is as follows: Cut the positive and negative electrode sheets into a certain size through a mold, and then stack them through a semi-automatic stacking machine to prepare a battery cell; After the battery cell is welded with pole ears, packaged, injected, and aged, it is formed. After the formation is completed, the capacity, pulse performance, and cycle performance can be tested. The 1C discharge of the soft-pack batteries assembled with the positive electrode sheets prepared in Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, and Comparative Example 5 was tested (the discharge current was set to 1.0A, and the voltage range was 4.3-2.5V). The discharge curve is shown in the attached figure. Figure 5 As shown in the attached Figure 5 It can be seen that the discharge capacity of the positive electrode sheet-assembled soft-pack batteries prepared in Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 at 1C rate is about 1.05Ah, the single cell is about 45g, and the specific energy is 90Wh / kg.

[0076] The 100C pulse discharge of the positive electrode sheet assembled soft-pack battery prepared in Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 (the discharge current is set to 100A, the voltage range is 4.3-2.5V, the pulse width is 1s, and the interval is 2s). The discharge curve is shown in the attached figure. Figure 6 As shown in the attached Figure 6 It can be seen that the positive electrode sheets assembled into soft-pack batteries prepared in Example 1 and Example 2 can withstand 39 and 37 pulse discharges respectively under the 100C pulse discharge condition, and the cut-off voltage is greater than the discharge lower limit voltage of 2.5V, while the positive electrode sheets assembled into soft-pack batteries prepared in Comparative Examples 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 have a discharge number less than 35 times under the 100C pulse discharge condition when the discharge voltage is less than 2.5V, indicating that the positive electrode sheets assembled into soft-pack batteries prepared in Example 1 and Example 2 have better 100C pulse discharge performance.

[0077] The 500C pulse discharge of the positive electrode sheet assembled soft-pack battery prepared in Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 (discharge current is set to 500A, voltage range is 4.3-2.5V, pulse width is 1s, interval is 1s), and the discharge curve is as shown in the attached figure. Figure 7 As shown in the attached Figure 7 It can be seen that the positive electrode sheets assembled into soft-pack batteries prepared in Example 1 and Example 2 can withstand 7 and 6 pulse discharges respectively under the condition of 500C pulse discharge, and the cut-off voltage is greater than the lower discharge limit voltage of 2.5V, while the positive electrode sheets assembled into soft-pack batteries prepared in Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 can only withstand 5 discharges at most when the voltage is not less than 2.5V under the condition of 500C pulse discharge, indicating that the positive electrode sheets assembled into soft-pack batteries prepared in Example 1 and Example 2 have better 500C pulse discharge performance.

[0078] The 10C charge / 20C discharge cycle of the positive electrode sheet assembled soft-pack battery prepared in Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 (charging current is set to 10A, discharging current is 20A, and voltage range is 4.2-2.5V) is tested. The capacity retention rate is as shown in the attached Figure 8 As shown in the attached Figure 8 It can be seen that the number of cycles at which the 10C charge / 20C discharge cycle capacity retention rate of the positive electrode sheet assembled soft-pack batteries prepared in Example 1 and Example 2 reaches 80% is greater than 2000 times, while the number of cycles at which the 10C charge / 20C discharge cycle capacity retention rate of the positive electrode sheet assembled soft-pack batteries prepared in Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, and Comparative Example 5 reaches 80% is less than 2000 times, indicating that the 10C charge / 20C discharge cycle performance of the positive electrode sheet assembled soft-pack batteries prepared in Example 1 and Example 2 is better.

Claims

1. A method for preparing a positive electrode material for an ultra-high power pulse type energy storage device, characterized in that: The following steps are involved: S1. Place transition metal lithium intercalation oxides of micron-scale and nanometer-scale particle sizes in a high-energy ball mill at a mass ratio of 70-95:5-30, and add an appropriate amount of solvent to form a slurry; the high-energy ball mill is milled at a speed of 200-400 r / min for 2-6 hours to obtain a mixed positive electrode material of transition metal lithium intercalation oxides with a mixture of micron-scale and nanometer-scale particle sizes; S2. After fully stirring the prepared mixed positive electrode material, conductive agent and binder, add an organic solvent, stir again to make a spray slurry, spray the slurry evenly on the surface of the substrate by electrostatic spraying, and obtain the electrostatic spraying mixed material positive electrode material after drying.

2. The method for preparing the positive electrode material of the ultra-high power pulse type energy storage device according to claim 1, characterized in that: The transition metal lithium-embedded oxides include LiCoO2, LiMn2O4, LiFePO4, LiNi 1~x~y Co y Mn x O2 (NCM ternary material), LiNi 1~x~y Co y Al x O2 (NCA ternary material), LiM x Mn 2~x O4 (M is Fe or Co doped atoms) is a positive electrode material for lithium-ion batteries.

3. The method for preparing the positive electrode material of the ultra-high power pulse type energy storage device according to claim 2, characterized in that: The mass proportion of nano-scale particles in the mixture is 5-30%.

4. The method for preparing the positive electrode material of the ultra-high power pulse type energy storage device according to claim 3, characterized in that: The mass ratio of the stainless steel balls to the milled material in the high-energy ball mill is 3 to 5:

1.

5. The method for preparing the positive electrode material of the ultra-high power pulse type energy storage device according to claim 4, characterized in that: The mass ratio of the small diameter ball, the medium diameter ball and the large diameter ball in the stainless steel ball is 4-5:3-4:2, and the diameters of the large ball, the medium ball and the small ball are 20 mm, 10 mm and 5 mm respectively.

6. The method for preparing the positive electrode material of the ultra-high power pulse type energy storage device according to claim 5, characterized in that: S1: placing the mixed positive electrode material obtained by ball milling in a vacuum oven and drying it at a temperature of 60° C. to 80° C. for 12 to 24 hours.

7. The method for preparing the positive electrode material of the ultra-high power pulse type energy storage device according to claim 6, characterized in that: During the S2 electrostatic spraying, after the single-side spraying of the substrate surface is completed, the substrate surface is dried, and the other side of the substrate surface is treated in the same way.

8. The method for preparing the positive electrode material of the ultra-high power pulse type energy storage device according to claim 7, characterized in that: The conductive agent is CNTs and SP, the binder is PVDF, the added mass ratio of the mixed positive electrode material and CNTs, SP and PVDF is: 85-92.5:2.5-5:2.5-5:2.5-5; the organic solvent is N-methylpyrrolidone.

9. The method for preparing the positive electrode material of the ultra-high power pulse type energy storage device according to claim 8, characterized in that: Inject the spray slurry into the spray gun of the electrostatic spray equipment, adjust the spray distance to 5-20 cm, the spray speed to 1-3 cm / s, set the electrostatic spray voltage to 10-20 kV, the ambient temperature to 25°C, and spray the spray slurry evenly on the surface of the substrate with a spray thickness of 15-35 μm.

10. The positive electrode material obtained according to the method for preparing positive electrode material for ultra-high power pulse type energy storage device according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Pole piece, energy storage device and preparation method of pole piece

    CN104600243A

  • Lithium-rich material / conductive organic polymer composite positive material and electrode preparation method

    CN108461719A

  • Preparation method of battery dry pole piece

    CN113611814A

  • Mixed positive electrode material, positive electrode plate and preparation method thereof, battery, and apparatus

    US20220359874A1