High-rate lithium iron phosphate positive electrode material as well as preparation method and application thereof
By coating the hyperbranched conductive polymer containing polyaniline segments on the lithium iron phosphate positive electrode material, the problem of low diffusion rate of lithium ion is solved, the rate performance and stability are improved, and the thermal stability and use are achieved life.
Patent Information
- Application Number
- CN202411412631.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-29
AI Technical Summary
The lithium iron phosphate positive electrode material has low lithium ion diffusion rate and low electronic conductivity, resulting in poor rate performance of lithium iron phosphate batteries, limiting its application range.
The hyperbranched conductive polymer containing polyaniline segments is used as the coating of lithium iron phosphate positive electrode material, and the silicone chain is used as the molecular framework to form a three-dimensional conductive network to improve the diffusion rate and electron conductivity of lithium ions, and through Graft modification enhances the adhesion and thermal stability of the material.
It significantly improves the rate performance and stability of lithium iron phosphate positive electrode material, extends service life, and improves mechanical properties and chemical stability, adapts to the use requirements of harsh environments.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium iron phosphate batteries, and in particular relates to a high-rate lithium iron phosphate positive electrode material, a preparation method and an application thereof. Background Art
[0002] Lithium batteries have a long service life, high energy density, safety and environmental friendliness. They are excellent green alternative energy sources that can greatly alleviate the environmental pollution problems caused by the current energy crisis. As the cathode material of the new generation of lithium batteries, lithium iron phosphate has the advantages of abundant raw materials, low cost, stable structure and no environmental pollution, and has received extensive attention and research in various fields.
[0003] However, lithium iron phosphate positive electrode materials are limited by their own structure and have the disadvantages of low ion diffusion rate and low electronic conductivity. In order to solve this problem, most of the current carbon coating technology is used to process lithium iron phosphate positive electrode materials to improve the electronic conductivity of lithium iron phosphate. However, this method still cannot effectively solve the problem of low lithium ion diffusion coefficient in lithium iron phosphate, resulting in poor high current charge and discharge performance of the obtained lithium iron phosphate battery. The poor rate performance also limits the application range of lithium iron phosphate positive electrode materials. Summary of the invention
[0004] The object of the present invention is to provide a high-rate lithium iron phosphate positive electrode material, a preparation method and application thereof, so as to solve the problem of poor rate performance of lithium iron phosphate batteries.
[0005] The purpose of the present invention can be achieved through the following technical solutions: In a first aspect, the present invention provides a high-rate lithium iron phosphate positive electrode material, the surface of which is coated with a hyperbranched conductive polymer containing polyaniline segments; the hyperbranched conductive polymer has a siloxane chain as a molecular skeleton.
[0006] By adopting the above technical solution, the molecular structure of the polyaniline segment contains a large electronic conjugation system, which can provide conditions for the delocalization migration of lithium ions and free electrons, and carry out lithium removal / lithium insertion reactions at a certain potential, thereby increasing the diffusion rate of lithium ions, shortening the diffusion distance of lithium ions, and improving the diffusion performance of lithium ions in lithium iron phosphate positive electrode materials, so that the obtained positive electrode material has excellent electrical conductivity and electrochemical properties. However, after the polyaniline segment itself is composited with the lithium iron phosphate positive electrode material, it is not resistant to high temperatures, has poor thermal stability, and has poor adhesion to the lithium iron phosphate positive electrode material. During the long-term cycle charge and discharge process, polyaniline will gradually lose its conductive effect, thereby reducing the service life of the lithium iron phosphate positive electrode material. Therefore, the polyaniline segment is grafted and modified.
[0007] Specifically, the present invention provides a hyperbranched conductive polymer, which is grafted with polyaniline chain segments to provide the polymer with good conductivity and lithium ion diffusivity. At the same time, the polymer is a hyperbranched structure with a large number of terminal groups, which can significantly improve the adhesion of the conductive polymer on the surface of the positive electrode material, and can also interact to form a three-dimensional mesh conductive network on the surface of the positive electrode material. This more open network structure and more abundant channels can accelerate the migration speed of lithium ions, thereby improving the rate performance of the lithium iron phosphate positive electrode material; and the molecular chains of the hyperbranched polymer will not easily entangle, and the molecular skeleton uses a siloxane chain, so that the mechanical properties, chemical stability and thermal stability of the positive electrode material are significantly improved, which can protect the internal lithium iron phosphate material, and is not easy to directly contact with the electrolyte to cause side reactions to form dendrites, so that the cycle performance of the battery can be maintained, and the obtained positive electrode material can meet the use of some harsh environments.
[0008] Preferably, the raw materials of the lithium iron phosphate positive electrode material include lithium iron phosphate powder and hyperbranched conductive polymer in a mass ratio of 1:(0.15-0.25).
[0009] Preferably, the raw materials of the hyperbranched conductive polymer include amino-terminated hyperbranched polysiloxane and aniline in a mass ratio of 1:(2-3).
[0010] By adopting the above technical scheme, the present invention selects amino-terminated hyperbranched polysiloxane as the scaffold compound of the hyperbranched conductive polymer. On the one hand, a large number of amino-terminated groups can realize the graft polymerization of aniline on the hyperbranched polysiloxane; on the other hand, the bond length of the silicon-oxygen bond of the amino-terminated hyperbranched polysiloxane is relatively long. Compared with the carbon-oxygen bond, the bonds of its molecular chain are easy to rotate, the interaction force between molecules is relatively small, and the amino-terminated hyperbranched polysiloxane has high flexibility, which makes it easier to form a network structure in the process of coating the lithium iron phosphate positive electrode material, and easier to adapt to the changes of the lithium iron phosphate positive electrode material. After combining with the polyaniline segment, the conductive network is further optimized, and an effective electron conduction path is provided, so as to maintain good rate performance, mechanical properties and thermal stability for the positive electrode material.
[0011] Preferably, the hyperbranched conductive polymer is prepared according to the following method: Preparation of amino-terminated hyperbranched polysiloxane: adding an aminosilane coupling agent to a solvent, mixing uniformly, adding deionized water under a nitrogen atmosphere, raising the temperature to 50-60° C., refluxing for 4-5 hours, and removing impurities by rotary evaporation to obtain amino-terminated hyperbranched polysiloxane; Preparation of hyperbranched conductive polymer: add amino-terminated hyperbranched polysiloxane to the solvent, stir and dissolve, adjust the solution pH to 2-3, add aniline, add initiator in an ice water bath, stir and react for 6-10 hours, and finally obtain the hyperbranched conductive polymer by suction filtration, washing and drying.
[0012] Preferably, the mass ratio of aminosilane coupling agent to deionized water is 1:(0.09-0.11).
[0013] Preferably, the aminosilane coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane and γ-aminopropylmethyldimethoxysilane.
[0014] Preferably, during the preparation of the amino-terminated hyperbranched polysiloxane, the solvent comprises a combination of one or more of ethanol, methanol, isopropanol and butanol.
[0015] Preferably, the initiator comprises a combination of one or more of ammonium persulfate, ferric chloride, potassium permanganate, potassium dichromate and hydrogen peroxide.
[0016] Preferably, the added amount of the initiator is 3-6% of the mass of aniline.
[0017] Preferably, during the preparation of the hyperbranched conductive polymer, the solvent includes a combination of one or more of N,N-dimethylformamide, N,N-dimethylacetamide and deionized water.
[0018] By adopting the above technical scheme, the present invention adopts a hydrolysis polycondensation method to prepare an amino-terminated hyperbranched polysiloxane, and the molecular weight of the hyperbranched polysiloxane prepared in this way is controllable and the structure is more stable; further, under acidic conditions and the action of an initiator, aniline is connected to the amino-terminated group on the hyperbranched polysiloxane and a graft polymerization reaction occurs to obtain a polyaniline segment, thereby optimizing the conductive network of the conductive polymer, expanding the diffusion channels of free electrons and lithium ions, and enhancing the rate performance, service life and thermal stability of the positive electrode material.
[0019] Preferably, the raw materials of the lithium iron phosphate powder include a lithium source, a phosphorus source and an iron source in a molar ratio of (1.05-1.1):(0.9-1.1):1.
[0020] Preferably, the lithium source includes one or more combinations of lithium hydroxide, lithium acetate, lithium oxalate, lithium carbonate, lithium dihydrogen phosphate, lithium phosphate and lithium nitrate.
[0021] Preferably, the phosphorus source includes a combination of one or more of phosphoric acid, ammonium phosphate, diammonium phosphate and lithium phosphate.
[0022] Preferably, the iron source includes one or more combinations of ferric nitrate, ferric oxide, ferrous chloride, ferrous sulfate, ferrous acetate, ferric hydroxide, ferric carbonate and ferric sulfate.
[0023] More preferably, the lithium iron phosphate powder is prepared by a hydrothermal method.
[0024] In a second aspect, the present invention provides a method for preparing a high-rate lithium iron phosphate positive electrode material, comprising the following process steps: S1. Add a nonionic surfactant to the solvent, stir to dissolve, then add lithium iron phosphate powder, stir and disperse to obtain a premixed solution; S2. The pH value of the premixed liquid is adjusted to 6-8, and a hyperbranched conductive polymer is added. The mixture is stirred and reacted for 5-7 hours under a nitrogen atmosphere, wherein the reaction temperature is 20-30° C., and then washed, neutralized and dried to obtain a high-rate lithium iron phosphate positive electrode material.
[0025] Preferably, the mass ratio of the nonionic surfactant to the lithium iron phosphate powder is (0.1-0.2):1.
[0026] Preferably, the nonionic surfactant includes a combination of one or more of polyvinyl alcohol, octylphenoxy polyoxyethylene ether, nonylphenol polyoxyethylene ether, sorbitan monolaurate and polyoxyethylene (20) sorbitan monolaurate.
[0027] Preferably, the solvent in step S1 is N-methylpyrrolidone.
[0028] By adopting the above technical solution, lithium iron phosphate powder is added to a solvent containing a non-ionic surfactant, which can improve the dispersibility between lithium iron phosphate powders and reduce the problem of decreased conductivity and rate performance caused by agglomeration between powders. Subsequently, a hyperbranched conductive polymer is added, in which the amino polar groups can form a strong intermolecular interaction force with the lithium iron phosphate powder, improve the adhesion of the conductive polymer on the surface of the positive electrode material, improve the service life of the positive electrode material, and gradually form a conductive network structure on the surface of the positive electrode material, thereby improving the rate performance of the positive electrode material.
[0029] In a third aspect, the present invention provides an application of a high-rate lithium iron phosphate positive electrode material in a lithium battery, including the high-rate lithium iron phosphate positive electrode material prepared by the present invention.
[0030] Beneficial effects of the present invention: The present invention adopts a hyperbranched conductive polymer containing polyaniline segments to modify lithium iron phosphate powder, wherein the polyaniline segments can provide conditions for delocalized migration of lithium ions and free electrons, and the hyperbranched conductive polymer adopts a siloxane chain as a molecular skeleton. After combining with polyaniline, in addition to being able to optimize the formed three-dimensional conductive network, the mechanical properties of the material, the adhesion to the positive electrode material and the thermal stability can also be improved, so that the rate performance and stability of the lithium iron phosphate positive electrode material obtained in this way are significantly improved. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Preparation Example Preparation Example 1: A lithium iron phosphate powder is prepared according to the following method: Dissolve 40 g of ferric nitrate and 9.8 g of phosphoric acid in 250 mL of deionized water, then add 1.5 g of ascorbic acid, and stir to obtain a premixed solution; Take 2.4 g of lithium hydroxide and dissolve it in 50 mL of deionized water. Add it into the premixed solution and stir for 30 minutes under a nitrogen atmosphere to obtain a precursor mixture. The obtained precursor mixture was hydrothermally synthesized in a high-pressure reactor, wherein the reaction temperature was 170° C. and the reaction time was 4 h, and then washed, dried and ground to obtain lithium iron phosphate powder.
[0033] Preparation Example 2 Hyperbranched Conductive Polymer Preparation Example 2-1, a hyperbranched conductive polymer, prepared according to the following method: 40 g of γ-aminopropyltriethoxysilane was added to 50 mL of methanol solution, mixed evenly, and 4 g of deionized water was added under nitrogen atmosphere, the temperature was raised to 55° C., refluxed for 4 h, and impurities were removed by rotary evaporation to obtain amino-terminated hyperbranched polysiloxane; Take 20g of amino-terminated hyperbranched polysiloxane and add it to 250mL of N,N-dimethylformamide. After stirring and dissolving, adjust the pH value of the solution to 2, add 50g of aniline, add 2.5g of ammonium persulfate in an ice water bath, stir and react for 8h, and finally obtain a hyperbranched conductive polymer by filtration, washing and drying.
[0034] Preparation Example 2-2, a hyperbranched conductive polymer, is different from Preparation Example 2-1 only in that the amount of deionized water added is 3.6 g.
[0035] Preparation Example 2-3, a hyperbranched conductive polymer, is different from Preparation Example 2-1 only in that the amount of deionized water added is 4.4 g.
[0036] Preparation Example 2-4, a hyperbranched conductive polymer, is different from Preparation Example 2-1 only in that the amount of aniline added is 40 g.
[0037] Preparation Example 2-5, a hyperbranched conductive polymer, is different from Preparation Example 2-1 only in that the amount of aniline added is 60 g.
[0038] Preparation Example 2-6, a hyperbranched conductive polymer, is different from Preparation Example 2-1 only in that the amount of deionized water added is 2.8 g.
[0039] Preparation Example 2-7, a hyperbranched conductive polymer, is different from Preparation Example 2-1 only in that the amount of deionized water added is 5.2 g.
[0040] Preparation Example 2-8, a hyperbranched conductive polymer, is different from Preparation Example 2-1 only in that the amount of aniline added is 30 g.
[0041] Preparation Example 2-9, a hyperbranched conductive polymer, is different from Preparation Example 2-1 only in that the amount of aniline added is 70 g.
[0042] Preparation Example 2-10, a conductive polymer, prepared according to the following method: Take 20g of amino-terminated polydimethylsiloxane (average molecular weight of 1500) and add it to 250mL of N,N-dimethylformamide. After stirring and dissolving, adjust the pH value of the solution to 2, add 50g of aniline, add 2.5g of ammonium persulfate in an ice water bath, stir and react for 8h, and finally obtain a conductive polymer by suction filtration, washing and drying.
[0043] Preparation Example 2-11, a hyperbranched conductive polymer, is prepared according to the following method: Take 20g of amino-terminated hyperbranched polyamide (molecular weight of 800-1000) and add it to 250mL of N,N-dimethylformamide. After stirring and dissolving, adjust the pH value of the solution to 2, add 50g of aniline, add 2.5g of ammonium persulfate in an ice water bath, stir and react for 8h, and finally obtain a hyperbranched conductive polymer by suction filtration, washing and drying.
[0044] Preparation Example 2-12, a hyperbranched conductive polymer, is prepared according to the following method: 40 g of γ-aminopropyltriethoxysilane was added to 50 mL of methanol solution and mixed evenly. Under a nitrogen atmosphere, 4 g of deionized water was added, and the temperature was raised to 55° C. After reflux reaction for 4 hours, impurities were removed by rotary evaporation to obtain amino-terminated hyperbranched polysiloxane, i.e., hyperbranched conductive polymer.
[0045] Preparation Example 2-13, a conductive polymer, prepared according to the following method: Take 250 mL of N,N-dimethylformamide, adjust the pH value of the solution to 2, add 50 g of aniline, add 2.5 g of ammonium persulfate in an ice water bath, stir and react for 8 hours, and finally obtain a conductive polymer by suction filtration, washing and drying.
[0046] Example Example 1: A high-rate lithium iron phosphate positive electrode material is prepared according to the following method: S1. Take 100mL N-methylpyrrolidone, add 1g nonylphenol polyoxyethylene ether, stir to dissolve, then add 10g of lithium iron phosphate powder obtained in Preparation Example 1, stir and disperse to obtain a premixed solution; S2. The pH value of the premixed liquid was adjusted to 7, 2 g of the hyperbranched conductive polymer prepared in Preparation Example 2-1 was added, and the mixture was stirred and reacted for 6 h under a nitrogen atmosphere, wherein the reaction temperature was 25° C., and then washed, neutralized and dried to obtain a high-rate lithium iron phosphate positive electrode material.
[0047] Example 2, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the added amount of the hyperbranched conductive polymer prepared in Preparation Example 2-1 is 1.5 g.
[0048] Example 3, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the amount of nonylphenol polyoxyethylene ether added is 2 g, and the amount of the hyperbranched conductive polymer prepared in Preparation Example 2-1 added is 2.5 g.
[0049] Example 4, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-2.
[0050] Example 5, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-3.
[0051] Example 6, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-4.
[0052] Example 7, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-5.
[0053] Example 8, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-6.
[0054] Example 9, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-7.
[0055] Example 10, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-8.
[0056] Example 11, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-9.
[0057] Comparative Example Comparative Example 1, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the added amount of the hyperbranched conductive polymer prepared in Preparation Example 2-1 is 1 g.
[0058] Comparative Example 2, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the added amount of the hyperbranched conductive polymer prepared in Preparation Example 2-1 is 3.5 g.
[0059] Comparative Example 3, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of conductive polymer prepared in Preparation Example 2-10.
[0060] Comparative Example 4, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-11.
[0061] Comparative Example 5, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of the hyperbranched conductive polymer prepared in Preparation Example 2-12.
[0062] Comparative Example 6, a high-rate lithium iron phosphate positive electrode material, is different from Example 1 only in that the hyperbranched conductive polymer prepared in Preparation Example 2-1 is replaced by an equal amount of conductive polymer prepared in Preparation Example 2-13.
[0063] Comparative Example 7 is a high-rate lithium iron phosphate positive electrode material, which is different from Example 1 only in that the lithium iron phosphate powder is not modified, and only the lithium iron phosphate powder prepared in Preparation Example 1 is used as the positive electrode material.
[0064] Performance testing Sample preparation: The positive electrode material obtained in the embodiment and the comparative example was mixed with a conductive agent (conductive carbon black) and a binder (polyvinylidene fluoride) in a mass ratio of 7:2:1, and 0.05 g / mL of N-methyl-2-pyrrolidone was added to dilute the slurry, and the mixture was ground and coated on an aluminum foil, and dried at 80°C for 24 h to obtain a positive electrode sheet. In a nitrogen atmosphere, a 2032 button battery was prepared using a lithium sheet as the negative electrode material, a polypropylene microporous membrane as the diaphragm, and 1 mol / L LiPF6 as the electrolyte.
[0065] 1. In the voltage range of 2.5-4.2V, at a constant temperature of 25℃, the specific capacity of the sample battery was tested at different rates of 1C, 5C, 10C and 20C; 2. Carry out charge and discharge cycle test on sample batteries in the voltage range of 2.5-4.2V, 1C rate and constant temperature of 25℃. The number of cycle tests is 100 and 200 cycles respectively. 3. The specific capacity of the test sample battery after 100 cycles at a voltage range of 2.5 to 4.2 V, a rate of 1C, and a constant temperature of 45°C.
[0066] The above test results are shown in Table 1, Table 2 and Table 3:
[0067]
[0068]
[0069]
[0070] According to Table 1, Table 2 and Table 3, combined with Example 1, Example 2 to Example 7, it can be seen that the specific capacity of Example 2 to Example 7 at different rates, different cycle times and different temperatures is not much different from that of Example 1. The only change of Example 2 to Example 7 compared with Example 1 is that the raw materials and the raw material ratio are adjusted within the required range, which has little effect on the final positive electrode material and lithium battery performance.
[0071] Combining Example 1, Example 8 to Example 11, it can be seen that the specific capacity of Example 8 to Example 11 is reduced compared with Example 1, and the specific capacity decreases with the increase of rate, the increase of cycle period and the increase of temperature. Example 8 to Example 11 mainly adjusts the raw material ratio of the hyperbranched conductive polymer used, wherein the amount of deionized water added in Example 8 is reduced, the molecular weight of the obtained hyperbranched conductive polymer decreases, the branching structure is reduced, the density of the formed conductive network decreases, the improvement effect on the lithium ion diffusion performance decreases, and the obtained lithium battery rate performance and electrochemical performance decrease; in Example 9, the amount of deionized water added is increased, and the molecular weight of the corresponding hyperbranched conductive polymer is large. During the coating process, the molecular chains are stacked, and the number of channels provided is reduced, which affects the conductive properties of the material. In Example 10, the amount of aniline added is reduced, the polyaniline segments on the hyperbranched conductive polymer are reduced, and the conductive properties decrease accordingly. In Example 11, the amount of aniline added is increased. The excessive molecular weight is not conducive to the coating modification of lithium iron phosphate powder, and the obtained particle size is too large, and the conductive properties and rate performance will also decrease accordingly.
[0072] Combined with Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 7, it can be seen that the specific capacity of Comparative Example 1, Comparative Example 2 and Comparative Example 7 is reduced compared with Example 1, and the specific capacity decreases with the increase of rate, the increase of cycle period and the increase of temperature, wherein the performance of Comparative Example 7 is significantly reduced compared with Example 1. Comparative Example 1, Comparative Example 2 and Comparative Example 7 are all adjusted in the amount of hyperbranched conductive polymer added compared with Example 1. Specifically, the amount of hyperbranched conductive polymer added is reduced in Comparative Example 1, resulting in a decrease in the content of conductive polymer coated on the surface of the obtained lithium iron phosphate positive electrode material. In addition to causing a decrease in the conductive performance of the positive electrode material, it is also not conducive to the formation of a conductive network, and the effect of improving thermal stability is also reduced. In Comparative Example 7, the lithium iron phosphate positive electrode material is not modified, and the conductive performance and rate performance are significantly reduced. In Comparative Example 2, the amount of hyperbranched conductive polymer added is increased, and the number of polymers coated on the lithium iron phosphate positive electrode material increases, which will affect the structure and particle size of the lithium iron phosphate itself, but is not conducive to the improvement of the electrochemical performance of the material.
[0073] Combined with Example 1, Comparative Examples 3 to 6, it can be seen that the specific capacity of Comparative Examples 3 to 6 is reduced compared with Example 1, and the specific capacity decreases with the increase of the rate, the increase of the cycle period and the increase of the temperature. Among them, the specific capacity decrease of Comparative Examples 3, Comparative Examples 4 and Comparative Examples 6 at high temperatures increases significantly, and the specific capacity of Comparative Examples 3 and Comparative Examples 5 at different rates decreases significantly. Specifically, the conductive polymer used in Comparative Example 3 does not contain a branched structure, and the conductive network structure formed by the conductive polymer on the surface of the positive electrode material is loose, which is difficult to synergistically enhance the diffusion rate of lithium ions in the positive electrode material with the polyaniline segment, and the rate performance is significantly reduced. The branched polymer in Comparative Example 4 is not based on a siloxane chain as a molecular skeleton, and the thermal stability of polyester compounds and polyaniline is not as good as that of hyperbranched polysiloxane. Under high temperature conditions, during the cyclic charge and discharge process, the conductive polymer coated on the surface of the positive electrode material will gradually lose its conductive effect and the effect of improving the lithium ion diffusion performance, resulting in a decrease in the rate performance and service life of the obtained positive electrode material. In Comparative Example 5, the hyperbranched conductive polymer is not grafted with polyaniline segments, the conductive effect of the siloxane main chain is poor, and the conductive performance of the positive electrode material is significantly reduced. In Comparative Example 6, polyaniline is used to replace the hyperbranched conductive polymer. On the one hand, the conductive network structure formed is not as good as that of the hyperbranched conductive polymer, the diffusion efficiency of lithium ions is not significantly improved, and the rate performance is significantly reduced compared with Example 1. In addition, the thermal stability of polyaniline itself is poor, and it will gradually lose its conductive effect during high-temperature and long-term cyclic charge and discharge, resulting in a decrease in the electrochemical performance of the obtained positive electrode material.
[0074] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0075] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-rate lithium iron phosphate positive electrode material, characterized in that: The surface of the lithium iron phosphate positive electrode material is coated with a hyperbranched conductive polymer containing polyaniline chain segments; the hyperbranched conductive polymer uses a siloxane chain as a molecular skeleton.
2. The high-rate lithium iron phosphate positive electrode material according to claim 1, characterized in that: The raw materials of the lithium iron phosphate positive electrode material include lithium iron phosphate powder and hyperbranched conductive polymer in a mass ratio of 1: (0.15-0.25).
3. The high-rate lithium iron phosphate positive electrode material according to claim 1, characterized in that: The raw materials of the hyperbranched conductive polymer include amino-terminated hyperbranched polysiloxane and aniline in a mass ratio of 1:(2-3).
4. The high-rate lithium iron phosphate positive electrode material according to claim 3, characterized in that: The hyperbranched conductive polymer is prepared according to the following method: Preparation of amino-terminated hyperbranched polysiloxane: adding an aminosilane coupling agent to a solvent, mixing uniformly, adding deionized water under a nitrogen atmosphere, raising the temperature to 50-60° C., refluxing for 4-5 hours, and removing impurities by rotary evaporation to obtain amino-terminated hyperbranched polysiloxane; Preparation of hyperbranched conductive polymer: add amino-terminated hyperbranched polysiloxane to the solvent, stir and dissolve, adjust the solution pH to 2-3, add aniline, add initiator in an ice water bath, stir and react for 6-10 hours, and finally obtain the hyperbranched conductive polymer by suction filtration, washing and drying.
5. The high-rate lithium iron phosphate positive electrode material according to claim 4, characterized in that: The mass ratio of the aminosilane coupling agent to deionized water is 1:(0.09-0.11).
6. The high-rate lithium iron phosphate positive electrode material according to claim 4, characterized in that: The initiator includes one or more combinations of ammonium persulfate, ferric chloride, potassium permanganate, potassium dichromate and hydrogen peroxide.
7. The high-rate lithium iron phosphate positive electrode material according to claim 2, characterized in that: The raw materials of the lithium iron phosphate powder include a lithium source, a phosphorus source and an iron source in a molar ratio of (1.05-1.1):(0.9-1.1):
1.
8. A method for preparing a high-rate lithium iron phosphate positive electrode material according to any one of claims 1 to 7, characterized in that: The process steps include: S1. Add a nonionic surfactant to the solvent, stir to dissolve, then add lithium iron phosphate powder, stir and disperse to obtain a premixed solution; S2. The pH value of the premixed liquid is adjusted to 6-8, and a hyperbranched conductive polymer is added. The mixture is stirred and reacted for 5-7 hours under a nitrogen atmosphere, wherein the reaction temperature is 20-30° C., and then washed and dried to obtain a high-rate lithium iron phosphate positive electrode material.
9. The method for preparing a high-rate lithium iron phosphate positive electrode material according to claim 8, characterized in that: The mass ratio of the nonionic surfactant to the lithium iron phosphate powder is (0.3-0.6):
1.