Composite, composite lithium supplement agent, and preparation method and application of composite lithium supplement agent

By using a composite of Ni@Co@M metal aerogel combined with solid electrolyte in the positive electrode of lithium-ion battery, the composite lithium supplement agent is prepared, which solves the problem of irreversible loss of lithium resources and achieves low deliquency potential and high discharge capacity , improves the overall performance and structural stability of the battery.

CN119050369AActive Publication Date: 2024-11-29LIONGO (CHANGZHOU) NEW ENERGY CO LTD

Patent Information

Application Number
CN202411527001.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-11-29
Estimated Expiration
2044-10-30

AI Technical Summary

Technical Problem

The solid electrolyte interface film formed by existing lithium-ion batteries during charging results in irreversible loss of lithium resources, affecting the discharge capacity and efficiency of the battery. The existing lithium supplement additives are inefficient and may damage the structure of the positive electrode material.

Method used

The composite of Ni@Co@M metal aerogel and solid electrolyte is used to prepare a composite lithium supplement agent through high-temperature sintering and hydrothermal method to form an aerogel coating on the surface of lithium oxalate to improve catalytic activity and ion transport capability. , reduce interface response.

Benefits of technology

The low deliquency potential and high first-time charge and discharge specific capacity of lithium-ion batteries are achieved, which improves the overall performance and structural stability of the battery and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a compound, a composite lithium supplement agent and a preparation method and application of the composite lithium supplement agent. The compound comprises metal aerogel and a solid electrolyte, the metal aerogel is Ni-Co-M metal aerogel, and M is Mo or Fe; and the solid electrolyte is selected from lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide or lithium lanthanum titanium oxide. Taking the compound as a component of an aerogel coating layer, and forming a composite lithium supplement agent with lithium oxalate; and the Ni-Co-M multi-metal aerogel is used as the substrate, so that the electrochemical performance of the lithium supplementing agent is improved. The solid electrolyte can increase the ionic conductivity and the electronic conductivity of the lithium oxalate, and after the lithium oxalate is decomposed, the solid electrolyte can also be used as a reaction product to improve the interface stability between the positive electrode and the electrolyte and improve the overall performance of the battery. The lithium ion battery prepared from the composite lithium supplement agent is relatively low in lithium removal potential and relatively high in first charge-discharge specific capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a composite material, a composite lithium supplement, and a preparation method and application thereof. Background Art

[0002] During the charging process of a standard lithium-ion battery, a solid electrolyte interface (SEI) film is formed on the surface of the negative electrode. This process consumes the active lithium released from the positive electrode, causing irreversible loss of some lithium resources, which in turn affects the overall performance of the battery, manifested as a decrease in the initial charging efficiency of the battery and a reduction in the discharge capacity. Therefore, improving the discharge capacity of the battery positive electrode and the transmission capacity of lithium ions has become the focus of research.

[0003] To address this challenge, current research focuses on adding lithium replenishing additives to cathode materials. These additives are designed to replenish consumed lithium ions without destroying the structure of the cathode material to increase the discharge capacity of the battery. However, existing lithium replenishing additives face multiple challenges, such as insufficient lithium replenishment, low efficiency, and possible negative impacts on the structural stability of the cathode material. These limitations hinder the widespread use of lithium replenishing additives in actual battery manufacturing.

[0004] Patent application CN117559013A uses a lithium replenishing agent and a conductor to form a lithium replenishing agent composite material. By adding the lithium replenishing agent composite material to the positive electrode of the battery, the lithium replenishing effect on the positive electrode is achieved during the battery charging and discharging process, effectively improving the discharge specific capacity of the positive electrode of the battery. However, the byproducts of the lithium replenishing agent used in the patent decompose during the cycle process will aggravate the interface side reaction between the electrode liquid and the positive electrode, resulting in reduced cycle performance. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a composite material, a composite lithium supplement, a preparation method and application thereof. The composite lithium supplement is prepared using the composite material, and the lithium ion battery finally prepared has a low delithiation potential and a high initial charge and discharge specific capacity.

[0006] The present invention provides a composite material, comprising a metal aerogel and a solid electrolyte; The metal aerogel is Ni@Co@M metal aerogel, where M is Mo or Fe; The solid electrolyte is selected from lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide or lithium lanthanum titanium oxide.

[0007] Preferably, the composite is obtained by sintering a mixture of a solid electrolyte precursor solution and a metal aerogel at high temperature.

[0008] Preferably, the method for preparing the mixture comprises the following steps: The solid electrolyte precursor solution is mixed with the metal aerogel and dried to obtain a mixture.

[0009] Preferably, the high temperature sintering includes: The mixture is heated to 700-900° C. and kept warm, and then heated to 1000-1200° C. and kept warm; The high-temperature sintering is performed under a protective gas atmosphere.

[0010] Preferably, the heating rate to 700-900°C is 0.5-5°C / min, and the holding time at 700-900°C is 3-6 h; The heating rate for reheating to 1000~1200℃ is 1~4℃ / min, and the holding time at 1000~1200℃ is 5~10 h.

[0011] Preferably, the preparation method of the Ni@Co@M metal aerogel comprises the following steps: An aqueous solution containing a structure directing agent and a complexing agent, a cobalt source, a nickel source, an M source and a reducing agent are mixed, deoxygenated, heated and stirred at 40-80° C. to form a hydrogel, and dried or solvent replaced to obtain a Ni@Co@M metal aerogel; the M source is a Mo source or a Fe source.

[0012] Preferably, the structure directing agent comprises at least one of a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, hexadecyltrimethylammonium bromide and a polyoxyethylene polyoxypropylene ether block copolymer; The complexing agent includes at least one of sodium citrate, nitrilotriacetic acid, ethylenediaminetetraacetic acid and adenosine triphosphate; The mass ratio of the structure directing agent to the complexing agent is (40-80): (60-120); In the aqueous solution containing the structure directing agent and the complexing agent, the mass ratio of the total mass of the structure directing agent and the complexing agent to water is 1:(15-25).

[0013] Preferably, the cobalt source includes at least one of cobalt acetate, cobalt acetylacetonate and cobalt nitrate; The nickel source includes nickel acetate and / or nickel nitrate; The Mo source includes molybdenum acetate dimer and / or ammonium molybdate; The Fe source includes ferric nitrate and / or ferric acetylacetonate; The reducing agent includes at least one of dimethylamine borane, sodium borohydride, ascorbic acid and metal organic framework MOFs.

[0014] Preferably, the mass ratio of the structure directing agent, complexing agent, cobalt salt, nickel salt, M source and reducing agent is (40-80): (60-120): (100-150): (100-150): (100-150): (800-1000).

[0015] The present invention also provides a composite lithium supplement, comprising: Lithium oxalate; An aerogel coating layer formed on the surface of the lithium oxalate; The component of the aerogel coating layer is the composite material described above.

[0016] The present invention also provides a method for preparing the composite lithium supplement agent described above, comprising the following steps: A) Grinding the aqueous solution of lithium oxalate to obtain nano-Li2C2O4; B) The composite and the nano-Li2C2O4 are uniformly dispersed in deionized water, and after ultrasonic treatment, a hydrothermal reaction is performed to obtain a composite lithium supplement.

[0017] Preferably, in step B), the mass ratio of the composite to the nano-Li2C2O4 is 1:(3-9); The power of the ultrasonic treatment is 500-3000 W, and the time is 0.5-5 h; The temperature of the hydrothermal reaction is 140-220° C., and the time is 6-24 h.

[0018] The present invention also provides a lithium ion battery, wherein the positive electrode of the lithium ion battery comprises a composite lithium supplement; The composite lithium supplement is the composite lithium supplement described above, or is the composite lithium supplement prepared by the preparation method described above.

[0019] The present invention provides a composite material, comprising a metal aerogel and a solid electrolyte; the metal aerogel is Ni@Co@M metal aerogel, M is Mo or Fe; the solid electrolyte is selected from lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide or lithium lanthanum titanium oxide. The composite material is used as a component of an aerogel coating layer to form a composite lithium supplement with lithium oxalate. The present invention first prepares Ni@Co@M metal aerogel, and then synthesizes a solid electrolyte in situ on the Ni@Co@M metal aerogel by high-temperature sintering to form a solid electrolyte catalyst (i.e., a composite material). Finally, the solid electrolyte catalyst is coated on nano lithium oxalate by a hydrothermal method to form a composite lithium oxalate lithium supplement. A new idea is proposed for the application of lithium oxalate lithium supplement.

[0020] Compared with the commonly used lithium supplements such as Li5FeO4 and conventional lithium oxalate sacrificial lithium supplements in the market, the lithium supplement of the present invention uses Ni@Co@M multi-metal aerogel as a substrate for the first time, which can provide a high specific surface area and porous structure, which helps to increase the metal sites of the catalyst. A large number of metal sites have high catalytic activity, which helps to promote the decomposition of lithium oxalate and the release of active lithium, thereby improving the electrochemical performance of the lithium supplement. The solid electrolyte provides an ion transmission channel to increase the ionic conductivity and electronic conductivity of lithium oxalate. At the same time, after the decomposition of lithium oxalate, the solid electrolyte as a reaction product can improve the interface stability between the positive electrode and the electrolyte, reduce the interface reaction, thereby reducing the interface impedance and improving the overall performance of the battery. The lithium-ion battery prepared by the composite lithium supplement of the present invention has a low delithiation potential and a high initial charge and discharge specific capacity. DETAILED DESCRIPTION

[0021] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] The present invention provides a composite (solid electrolyte / Ni@Co@M aerogel), comprising a metal aerogel and a solid electrolyte; The metal aerogel is Ni@Co@M metal aerogel, where M is Mo or Fe; The solid electrolyte is selected from lithium aluminum titanium phosphate (LATP), lithium lanthanum zirconium oxide (LLZO) or lithium lanthanum titanium oxide (LLTO).

[0023] The composite is obtained by sintering a mixture of a solid electrolyte precursor solution and a metal aerogel at high temperature.

[0024] In certain embodiments of the present invention, the method for preparing the mixture comprises the following steps: The solid electrolyte precursor solution is mixed with the Ni@Co@M metal aerogel and dried to obtain a mixture.

[0025] In certain embodiments of the present invention, the method for preparing the Ni@Co@M metal aerogel comprises the following steps: An aqueous solution containing a structure directing agent and a complexing agent, a cobalt source, a nickel source, an M source and a reducing agent are mixed, deoxygenated, heated and stirred at 40-80° C. to form a hydrogel, and dried or solvent replaced to obtain a Ni@Co@M metal aerogel; the M source is a Mo source or a Fe source.

[0026] The structure directing agent is at least one of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123), hexadecyl trimethyl ammonium bromide (CTAB) and polyoxyethylene polyoxypropylene ether block copolymer (F127). The complexing agent is at least one of sodium citrate, nitrilotriacetic acid, ethylenediaminetetraacetic acid and adenosine triphosphate. The mass ratio of the structure directing agent to the complexing agent is 40~80:60~120, such as 40:60, 40:120, 80:120. In the aqueous solution containing the structure directing agent and the complexing agent, the mass ratio of the total mass of the structure directing agent and the complexing agent to the water is 1:15~25, such as 1:20, 1:25. The solvent of the aqueous solution containing the structure directing agent and the complexing agent is deionized water.

[0027] The cobalt source is at least one of cobalt acetate, cobalt acetylacetonate and cobalt nitrate. The nickel source is nickel acetate and / or nickel nitrate. The Mo source is molybdenum acetate dimer and / or ammonium molybdate. The Fe source is ferric nitrate and / or ferric acetylacetonate. The reducing agent is at least one of dimethylamine borane, sodium borohydride, ascorbic acid and metal organic framework MOFs.

[0028] The mass ratio of the structure directing agent, complexing agent, cobalt salt, nickel salt, M source and reducing agent is 40~80:60~120:100~150:100~150:100~150:800~1000, for example, 40:60:100:100:100:800, 40:120:100:125:150:1000, 80:120:100:125:150:900.

[0029] The deoxygenation method comprises: The mixture is evacuated and replaced with an inert gas to remove dissolved oxygen in the mixed solution and protect the prepared sample from oxidation. The inert gas may be Ar.

[0030] The heating and stirring time at 40-80° C. is 8-24 h. Specifically, the heating and stirring temperature is 40° C., 80° C., and the time is 24 h, 8 h.

[0031] In certain embodiments of the present invention, after the hydrogel is formed, the process further comprises: washing and transferring to an alcohol solution for reflux. Deionized water is used for washing. The reflux temperature is 30-60°C, such as 30°C; the time is 12-20 h, such as 12 h, 20 h. The purpose of transferring to an alcohol solution for reflux is to remove residues. The alcohol solution is methanol and / or ethanol. The drying method comprises freeze drying, supercritical drying, atmospheric pressure drying, vacuum drying or microwave drying.

[0032] After obtaining the Ni@Co@M metal aerogel, a solid electrolyte is synthesized in situ on the Ni@Co@M metal aerogel to obtain a composite (ie, solid electrolyte / Ni@Co@M aerogel).

[0033] Specifically, they include: The solid electrolyte precursor solution is mixed with the Ni@Co@M metal aerogel, dried, and then a mixture is obtained and sintered at a high temperature.

[0034] In certain embodiments of the present invention, the mass ratio of the solid electrolyte precursor solution to the Ni@Co@M metal aerogel is 20-50:1, such as 20:1, 50:1, or 30:1.

[0035] In certain embodiments of the present invention, the solid electrolyte precursor solution is a LATP precursor solution, a LLZO precursor solution or a LLZTO precursor solution.

[0036] In certain embodiments of the present invention, the LATP precursor solution is obtained by stirring and mixing LiNO3, Al(NO3)3·9H2O, Ti(OC4H9)4, NH4H2PO4, citric acid and water at 30-70° C. The mass ratio of LiNO3, Al(NO3)3·9H2O, Ti(OC4H9)4, NH4H2PO4 and citric acid is 90-105:150-250:480-620:240-360:960-1200, such as 90:150:480:240:960, 105:250:620:360:1200, 95:200:540:300:1080. The present invention has no special restrictions on the amount ratio of the water, which can dissolve LiNO3, Al(NO3)3·9H2O, Ti(OC4H9)4, NH4H2PO4 and citric acid. The stirring and mixing temperature is 60°C, 70°C, 50°C; the rotation speed is 100-400 rpm, such as 100 rpm, 400 rpm, 150 rpm; the time is 30-240 min, such as 120 min, 240 min, 160 min. The water is deionized water.

[0037] The drying temperature is 50-80°C and the drying time is 20-48 hours.

[0038] In some embodiments of the present invention, the high temperature sintering comprises: The mixture is heated to 700-900° C. and kept warm, and then heated to 1000-1200° C. and kept warm; The high-temperature sintering is performed under a protective gas atmosphere.

[0039] In some embodiments of the present invention, the protective gas is nitrogen.

[0040] Before heating the mixture to 700-900° C., the method further comprises: introducing protective gas at a flow rate of 0.5-2 m³ / h, specifically, the flow rate is 0.5 m³ / h, 2 m³ / h, and 1 m³ / h. The heating and heat preservation are both performed in an atmosphere furnace.

[0041] In certain embodiments of the present invention, the heating rate to 700-900°C is 0.5-5°C / min, such as 0.5°C / min, 5°C / min, 2.5°C / min. The holding time at 700-900°C is 3-6 h, such as 6 h, 3 h, 4 h. Specifically, the temperature is 700°C, 900°C, or 800°C.

[0042] In certain embodiments of the present invention, the heating rate of reheating to 1000-1200°C is 1-4°C / min, such as 1°C / min, 4°C / min, 2°C / min. The time of keeping at 1000-1200°C is 5-10 h, such as 10 h, 5 h, 6 h. Specifically, reheating to 1000°C, 1200°C, 1100°C. After reheating to 1000-1200°C and keeping, it also includes: naturally cooling to room temperature.

[0043] The present invention also provides a composite lithium supplement, comprising: Lithium oxalate; An aerogel coating layer formed on the surface of the lithium oxalate; The component of the aerogel coating layer is the composite material described above.

[0044] The lithium oxalate is nano lithium oxalate.

[0045] The aerogel coating layer is obtained by in-situ synthesis of solid electrolyte from Ni@Co@M metal aerogel.

[0046] Specifically, the aerogel coating layer is obtained by sintering a mixture of a solid electrolyte precursor solution and a metal aerogel at a high temperature.

[0047] In the present invention, an aerogel coating layer (ie, a solid electrolyte / Ni@Co@M aerogel coating layer) is formed on the surface of nano lithium oxalate by a hydrothermal method.

[0048] The present invention also provides a method for preparing the composite lithium supplement agent described above, comprising the following steps: A) Grinding the aqueous solution of lithium oxalate to obtain nano-Li2C2O4; B) The composite and the nano-Li2C2O4 are uniformly dispersed in deionized water, and after ultrasonic treatment, a hydrothermal reaction is performed to obtain a composite lithium supplement.

[0049] In step A): After grinding the aqueous solution of lithium oxalate, nano-Li2C2O4 is obtained.

[0050] In certain embodiments of the present invention, the solvent in the aqueous solution of lithium oxalate is deionized water. In the aqueous solution of lithium oxalate, the mass ratio of lithium oxalate to deionized water is 1:5-10, such as 1:10, 1:5. The grinding is performed in a sand mill. The grinding speed is 500-2500 rpm, such as 500 rpm, 2500 rpm; the grinding time is 2-8 h, such as 8 h, 2 h.

[0051] In step B): The composite (solid electrolyte / Ni@Co@M aerogel) and the nano-Li2C2O4 are uniformly dispersed in deionized water, and after ultrasonic treatment, a hydrothermal reaction is performed to obtain a composite lithium supplement; The solid electrolyte / Ni@Co@M aerogel is obtained by high-temperature sintering of a Ni@Co@Mo metal aerogel in which pores are filled with a solid electrolyte precursor.

[0052] In certain embodiments of the present invention, the mass ratio of the composite (solid electrolyte / Ni@Co@M aerogel) to the nano-Li2C2O4 is 1:3~9, such as 1:9, 1:3, 1:7. The power of the ultrasonic treatment is 500~3000 W, such as 3000W, 2500 W; the time is 0.5~5 h, such as 0.5 h, 1 h. The temperature of the hydrothermal reaction is 140~220℃, such as 140℃, 220℃, 200℃; the time is 6~24 h, such as 24 h, 6 h, 8 h; the hydrothermal reaction is carried out in a polytetrafluoroethylene-lined pressure reactor.

[0053] In the composite lithium supplement obtained by the present invention, the solid electrolyte / Ni@Co@M aerogel is coated with nano lithium oxalate.

[0054] The present invention also provides a lithium ion battery, wherein the positive electrode of the lithium ion battery comprises a composite lithium supplement; the composite lithium supplement is the composite lithium supplement described above, or a composite lithium supplement prepared by the preparation method described above.

[0055] The lithium ion battery can be a button cell or a soft pack cell.

[0056] When the lithium-ion battery is a button battery: The positive electrode of the lithium-ion battery is prepared by coating a positive electrode slurry including a positive electrode active material, a conductive agent, a binder and a solvent on a positive electrode current collector; the positive electrode active material is the composite lithium supplement agent described above, or the composite lithium supplement agent prepared by the preparation method described above.

[0057] The conductive agent is conductive carbon black (SP). The binder is polyvinylidene fluoride (PVDF). The solvent is N-methylpyrrolidone (NMP). The positive electrode current collector is aluminum foil.

[0058] In the positive electrode slurry, the mass ratio of the positive electrode active material, the conductive agent and the binder is 84-87:8-12:3-7, such as 85:10:5. The solid content of the positive electrode slurry is 20%-35%, such as 25%.

[0059] In certain embodiments of the present invention, the method for preparing the positive electrode of the lithium ion battery comprises the following steps: After the positive electrode active material, conductive agent, binder and solvent are mixed evenly, the obtained mixed slurry is coated on the positive electrode collector, and after drying, the mixed slurry is rolled and punched to obtain a positive electrode sheet.

[0060] The coating thickness is 100-250 μm, for example 250 μm. The positive electrode current collector is aluminum foil.

[0061] The drying temperature is 100-140° C. and the drying time is 10-14 h.

[0062] When the lithium-ion battery is a button battery, the negative electrode is a lithium sheet; the separator is a polypropylene porous membrane, specifically a celgard2400 polypropylene porous membrane; the electrolyte is a 1 mol / L LiPF6 solution, and the solvent is ethylene carbonate (EC) and dimethyl carbonate (DMC), with a volume ratio of 1:1. The button battery is assembled in a glove box filled with argon gas, the water oxygen value in the glove box is controlled to be less than 0.01 ppm, and the battery is pressurized and sealed with a sealing machine to obtain a button battery.

[0063] When the lithium-ion battery is a soft-pack battery: The positive electrode of the lithium-ion battery is prepared by coating a positive electrode slurry including a positive electrode active material, a binder, a conductive agent, a lithium supplement agent and a solvent on the surface of a positive electrode current collector; the lithium supplement agent is the composite lithium supplement agent described above, or the composite lithium supplement agent prepared by the preparation method described above.

[0064] The positive electrode active material is a single crystal high nickel ternary material or lithium iron phosphate. The single crystal high nickel ternary material is LiNi 0.92 Co 0.055 Mn 0.25O2. The binder is a PVDF NMP solution with a mass concentration of 1% to 2%; or the binder is PVDF. The conductive agent is conductive carbon black (SP). The positive electrode current collector is aluminum foil with a thickness of 20 μm.

[0065] The mass ratio of the single crystal high nickel ternary material, the binder, the conductive agent and the lithium supplement agent is 94:3:1.5:1.5. The solid content of the positive electrode slurry is 40% to 60%, for example, 50%.

[0066] In certain embodiments of the present invention, the negative electrode of the lithium-ion battery is a graphite negative electrode. Or the negative electrode of the lithium-ion battery is prepared by coating a negative electrode slurry including silicon-carbon negative electrode 1800 (Cruder), conductive agent Super P, thickener (deionized aqueous solution of sodium carboxymethyl cellulose CMC), binder (deionized aqueous solution of styrene-butadiene rubber SBR), deionized aqueous solution of polyacrylic acid PAA and deionized aqueous solution of single-walled carbon nanotube CNT on the surface of the negative electrode current collector.

[0067] In certain embodiments of the present invention, the method for preparing the positive electrode of the lithium ion battery comprises the following steps: After uniformly mixing the single crystal high nickel ternary material, the binder, the conductive agent, the lithium supplement agent and the solvent, the obtained mixed slurry is coated on the surface of the positive electrode collector, and after drying, the positive electrode sheet is obtained.

[0068] The single-side thickness of the coating is 100-250 μm, such as 246 μm. The coating speed is 0.5-1.5 m / min, such as 1 m / min. The coating on the surface of the positive electrode current collector can be coated on both sides of the positive electrode current collector. The drying temperature is 140-150°C.

[0069] The positive electrode sheet is roll-pressed, the electrode tabs are welded, and the positive electrode sheet is paired with a graphite negative electrode to prepare a soft-pack battery.

[0070] Or the positive electrode sheet and the negative electrode sheet are rolled separately, and the tabs are welded to prepare a soft-pack battery; the negative electrode sheet is prepared by uniformly coating a negative electrode slurry including a silicon-carbon composite material, a conductive agent, a thickener, a binder, a polyacrylic acid solution and a single-walled carbon nanotube solution on a negative electrode collector (copper foil).

[0071] The design voltage of the soft-pack battery is 3~4.25 V and the design capacity is 2.5 Ah.

[0072] The present invention directly prepares a Ni@Co@M metal aerogel catalyst (composite) filled with a solid electrolyte, which provides a large number of active sites and specific surface area, helps to improve the efficiency of the catalytic reaction and promotes the decomposition reaction of lithium oxalate. At the same time, the conductive properties of the metal aerogel help to improve the electron transfer efficiency of the battery, thereby improving the overall performance of the battery. In addition, the filling of the solid electrolyte enhances the structural integrity of the metal aerogel, making it more resistant to mechanical stress during the battery cycle, which helps to ensure the structural stability of the catalyst.

[0073] The present invention coats the surface of nano lithium oxalate with solid electrolyte / Ni@Co@M aerogel to form a composite lithium oxalate lithium supplement. The large number of active sites and specific surface area of ​​the catalyst can reduce the decomposition potential of lithium oxalate, so that the lithium supplement can be quickly decomposed at a voltage of 4V, replenishing a large amount of active lithium for the battery system. At the same time, after the lithium oxalate is decomposed, the remaining reaction product is Ni@Co@Mo metal aerogel filled with solid electrolyte. The reaction product has both the additional ion channels of the solid electrolyte and the high electronic conductivity of the metal aerogel, which can greatly improve the ionic conductivity and electronic conductivity inside the battery, reduce the internal resistance of the battery system, reduce the heat loss of the battery during the charge and discharge process, and help reduce the increase in battery temperature, thereby reducing the speed of battery aging and extending the service life of the battery.

[0074] The present invention has no particular limitation on the sources of the raw materials used above, and they can be generally commercially available.

[0075] In order to further illustrate the present invention, the composite material, the composite lithium supplement, the preparation method and the application thereof provided by the present invention are described in detail below in combination with the examples, but they should not be construed as limiting the scope of protection of the present invention.

[0076] Example 1 1) Preparation of Ni@Co@Mo metal aerogel: In a flask, 40g of P123 and 60g of sodium citrate were completely dissolved in deionized water, and the mass ratio of the total mass of P123 and sodium citrate to the deionized water was 1:20. Then, 100g of cobalt acetate, 100g of nickel acetate, 100g of molybdenum acetate dimer and 800g of dimethylamine borane were added in sequence. The flask containing the above solution was evacuated and replaced with inert gas Ar to remove dissolved oxygen in the solution and protect the prepared sample from oxidation. After that, it was heated and stirred at 40°C for 24h to form a hydrogel. The obtained hydrogel was washed with deionized water, transferred to ethanol, and refluxed at 30°C for 12h to remove the residue. Finally, Ni@Co@Mo metal aerogel was obtained by freeze drying.

[0077] 2) Preparation of Ni@Co@Mo aerogel (mixture) with pores filled with LATP precursor: 90 g of LiNO3, 150 g of Al(NO3)3·9H2O, 480 g of Ti(OC4H9)4, 240 g of NH4H2PO4 and 960 g of citric acid were weighed, then dissolved in 5 L of deionized water, and stirred at 60°C and 100 rpm for 120 min to obtain a uniformly mixed LATP precursor solution; the LATP precursor solution was poured into the Ni@Co@Mo aerogel (the mass ratio of the LATP precursor solution to the Ni@Co@Mo aerogel was 20:1) to fill the LATP precursor solution into the pores of the Ni@Co@Mo aerogel, and dried at 50°C for 48 h to obtain a Ni@Co@Mo metal aerogel with the pores filled with the LATP precursor.

[0078] 3) High temperature sintering to obtain LATP / Ni@Co@Mo aerogel (composite): The Ni@Co@Mo metal aerogel with LATP precursor in the pores was placed in an atmosphere furnace, nitrogen was introduced at a flow rate of 0.5 m³ / h, the temperature was increased to 700°C at a heating rate of 0.5°C / min, and the temperature was kept for 6 h. Then the temperature was increased to 1000°C at a heating rate of 1°C / min, and the temperature was kept for 10 h. After naturally cooling to room temperature, LATP / Ni@Co@Mo aerogel was obtained.

[0079] 4) Preparation of composite lithium supplement: The lithium oxalate was evenly dispersed in deionized water at a mass ratio of 1:10, and then transferred to a sand mill and ground at 500rpm for 8h to obtain nano-Li2C2O4. The LATP / Ni@Co@Mo aerogel and the nano-Li2C2O4 were evenly dispersed in deionized water at a mass ratio of 1:9, and ultrasonically treated at 3000 W for 0.5h. Then, the mixed solution was transferred to a polytetrafluoroethylene-lined pressure reactor and hydrothermally reacted at 140°C for 24h to obtain a composite lithium supplement of LATP / Ni@Co@Mo aerogel-coated nano-lithium oxalate.

[0080] Comparative Example 1 The difference from Example 1 is that: Steps 2) and 3) are not included; In step 4): The lithium oxalate was evenly dispersed in deionized water, the mass ratio of lithium oxalate to deionized water was 1:10, and then transferred to a sand mill and ground at 500rpm for 8h to obtain nano-Li2C2O4. The Ni@Co@Mo metal aerogel and the nano-Li2C2O4 were evenly dispersed in deionized water at a mass ratio of 1:9, and ultrasonically treated at 3000 W for 0.5h. Then, the mixed solution was transferred to a polytetrafluoroethylene-lined pressure reactor and hydrothermally reacted at 140°C for 24h to obtain a composite lithium supplement of Ni@Co@Mo aerogel-coated nano-lithium oxalate.

[0081] Comparative Example 2 The difference from Example 1 is that the LATP / Ni@Co@Mo aerogel-coated lithium oxalate is replaced by graphene oxide sheets and Co3O4 quantum dots-coated lithium oxalate: The lithium supplement additive includes lithium oxalate, Co3O4 quantum dots and graphene oxide sheets. The Co3O4 quantum dots are attached to part of the outer surface of the lithium oxalate, and the graphene oxide sheets are coated on the outer surfaces of the Co3O4 quantum dots and lithium oxalate. The particle size of lithium oxalate is 100nm, and the particle size of the Co3O4 quantum dots is 3nm. Among them, the graphene oxide sheets are connected by hydrogen bonds to form a three-dimensional conductive network. The graphene oxide sheets are porous structures. The mass ratio of lithium oxalate, Co3O4 quantum dots and graphene oxide is 80:10:10.

[0082] Example 2 1) Preparation of Ni@Co@Fe metal aerogel: In a flask, 40 g of CTAB and 120 g of nitrilotriacetic acid were completely dissolved in deionized water, and the mass ratio of the total mass of CTAB and nitrilotriacetic acid to the deionized water was 1:25. Then, 100 g of cobalt nitrate, 125 g of ferric nitrate, 150 g of nickel acetylacetonate and 1000 g of sodium borohydride were added in sequence. Then, the flask containing the above solution was evacuated and replaced with inert gas Ar to remove dissolved oxygen in the solution and protect the prepared sample from oxidation. After that, it was stirred at 80 ° C for 8 h to form a hydrogel. The obtained hydrogel was washed with deionized water, transferred to methanol, and refluxed at 30 ° C for 20 h to remove the residue. Finally, Ni@Co@Fe metal aerogel was obtained by freeze drying.

[0083] 2) Preparation of Ni@Co@Fe aerogels with pores filled with LATP precursors: 105 g of LiNO3, 250 g of Al(NO3)3·9H2O, 620 g of Ti(OC4H9)4, 360 g of NH4H2PO4 and 1200 g of citric acid were weighed and dissolved in 6 L of deionized water, and stirred at 70°C and 400 rpm for 240 min to obtain a uniformly mixed LATP precursor solution; the LATP precursor solution was poured into the Ni@Co@Fe aerogel (the mass ratio of the LATP precursor solution to the Ni@Co@Fe aerogel was 50:1) to fill the LATP precursor solution into the pores of the Ni@Co@Fe aerogel, and dried at 80°C for 20 h to obtain a Ni@Co@Fe metal aerogel with the pores filled with the LATP precursor.

[0084] 3) High temperature sintering to obtain LATP / Ni@Co@Fe aerogel: The Ni@Co@Fe metal aerogel with LATP precursor in its pores was placed in an atmosphere furnace, nitrogen was introduced at a flow rate of 2 m³ / h, the temperature was increased to 900°C at a heating rate of 5°C / min, kept warm for 3 h, then increased to 1200°C at a heating rate of 4°C / min, kept warm for 5 h, and naturally cooled to room temperature to obtain LATP / Ni@Co@Fe aerogel.

[0085] 4) Preparation of composite lithium supplement: The lithium oxalate was evenly dispersed in deionized water at a mass ratio of 1:5, and then transferred to a sand mill and ground at 2500rpm for 2h to obtain nano-Li2C2O4. The LATP / Ni@Co@Fe aerogel and the nano-Li2C2O4 were evenly dispersed in deionized water at a mass ratio of 1:3, and ultrasonically treated at 3000 W for 0.5h. Then, the mixed solution was transferred to a polytetrafluoroethylene-lined pressure reactor and hydrothermally reacted at 220℃ for 6h to obtain a composite lithium supplement of LATP / Ni@Co@Fe aerogel-coated nano-lithium oxalate.

[0086] Comparative Example 3 The difference from Example 2 is that the LATP / Ni@Co@Fe aerogel catalyst coating is replaced by LATP coating: 1) Preparation of LATP precursor: Weigh 105 g of LiNO3, 250 g of Al(NO3)3·9H2O, 620 g of Ti(OC4H9)4, 360 g of NH4H2PO4 and 1200 g of citric acid, then dissolve in 6 L of deionized water, stir at 70 ° C and 400 rpm for 240 min to obtain a uniformly mixed LATP precursor solution, and dry at 80 ° C for 20 h to obtain a LATP precursor.

[0087] 2) High temperature sintering to obtain LATP aerogel: The LATP precursor was placed in an atmosphere furnace, heated to 900°C at a heating rate of 5°C / min, kept warm for 3 hours, then heated to 1200°C at a heating rate of 4°C / min, kept warm for 5 hours, and naturally cooled to room temperature to obtain LATP aerogel.

[0088] 3) Preparation of composite lithium supplement: The lithium oxalate was evenly dispersed in deionized water, the mass ratio of lithium oxalate to deionized water was 1:5, and then transferred to a sand mill and ground at 2500rpm for 2h to obtain nano-Li2C2O4. The LATP aerogel and the nano-Li2C2O4 were evenly dispersed in deionized water at a mass ratio of 1:3, and ultrasonically treated at 3000 W for 0.5h. Then, the mixed solution was transferred to a polytetrafluoroethylene-lined pressure reactor and hydrothermally reacted at 220°C for 6h to obtain a composite lithium supplement of LATP aerogel-coated nano-lithium oxalate.

[0089] Example 3 1) Preparation of Ni@Co@Mo metal aerogel: In a flask, 80g of F127 and 120g of adenosine triphosphate were completely dissolved in deionized water, and the mass ratio of the total mass of F127 and adenosine triphosphate to the deionized water was 1:20. Then, 100g of cobalt acetylacetonate, 125g of nickel acetate, 150g of ammonium molybdate and 900g of ascorbic acid were added in sequence. The flask containing the above solution was evacuated and replaced with inert gas Ar to remove dissolved oxygen in the solution and protect the prepared sample from oxidation. After that, it was heated and stirred at 80°C for 8h to form a hydrogel. The obtained hydrogel was washed with deionized water, transferred to ethanol, and refluxed at 30°C for 20h to remove the residue. Finally, Ni@Co@Mo metal aerogel was obtained by freeze drying.

[0090] 2) Preparation of Ni@Co@Mo aerogel with pores filled with LATP precursor: 95 g of LiNO3, 200 g of Al(NO3)3·9H2O, 540 g of Ti(OC4H9)4, 300 g of NH4H2PO4 and 1080 g of citric acid were weighed, then dissolved in 5 L of deionized water, and stirred at 50°C and 150 rpm for 160 min to obtain a uniformly mixed LATP precursor solution; the LATP precursor solution was poured into the Ni@Co@Mo aerogel (the mass ratio of the LATP precursor solution to the Ni@Co@Mo aerogel was 30:1) to fill the LATP precursor solution into the pores of the Ni@Co@Mo aerogel, and dried at 60°C for 36 h to obtain a Ni@Co@Mo metal aerogel with the pores filled with the LATP precursor.

[0091] 3) High temperature sintering to obtain LATP / Ni@Co@Mo aerogel: The Ni@Co@Mo metal aerogel with LATP precursor in the pores was placed in an atmosphere furnace, nitrogen was introduced at a flow rate of 1m³ / h, the temperature was increased to 800°C at a heating rate of 2.5°C / min, kept warm for 4h, then increased to 1100°C at a heating rate of 2°C / min, kept warm for 6h, and naturally cooled to room temperature to obtain LATP / Ni@Co@Mo aerogel.

[0092] 4) Preparation of composite lithium supplement: The lithium oxalate was evenly dispersed in deionized water at a mass ratio of 1:7, and then transferred to a sand mill and ground at 2000rpm for 3h to obtain nano-Li2C2O4. The LATP / Ni@Co@Mo aerogel and the nano-Li2C2O4 were evenly dispersed in deionized water at a mass ratio of 1:5, and ultrasonically treated at 2500 W for 1h. Then, the mixed solution was transferred to a polytetrafluoroethylene-lined pressure reactor and hydrothermally reacted at 200℃ for 8h to obtain a composite lithium supplement of LATP / Ni@Co@Mo aerogel-coated nano-lithium oxalate.

[0093] Comparative Example 4 The difference from Example 3 is: The LATP / Ni@Co@Mo aerogel coating is replaced by LATP / Ni@Co@Mo ordinary catalyst coating: 1) Preparation of conventional catalyst (Ni@Co@Mo catalyst): The total mass of 100g Ketjen black, 100g cobalt acetylacetonate, 125g nickel acetate, 150g ammonium molybdate and 900g ascorbic acid and deionized water were completely dissolved in deionized water at a mass ratio of 1:20, and the obtained solution was heated and stirred at 80°C for 8h, and dried in an oven at 100°C for 24h. Then, it was placed in an atmosphere furnace with N2 atmosphere, heated to 950°C at a heating rate of 2°C / min, kept warm for 3h, and naturally cooled to room temperature to obtain Ni@Co@Mo catalyst.

[0094] 2) Preparation of a mixture of LATP precursor and Ni@Co@Mo catalyst: 95 g of LiNO3, 200 g of Al(NO3)3·9H2O, 540 g of Ti(OC4H9)4, 300 g of NH4H2PO4 and 1080 g of citric acid were weighed, then dissolved in 5 L of deionized water, and stirred at 50°C and 150 rpm for 160 min to obtain a uniformly mixed LATP precursor solution; the Ni@Co@Mo catalyst was added to the LATP precursor solution (the mass ratio of the LATP precursor solution to the Ni@Co@Mo catalyst was 30:1), stirred at 60°C and 2000 rpm for 30 min, and then dried at 80°C for 36 h to obtain a mixture of the LATP precursor and the Ni@Co@Mo catalyst.

[0095] 3) High temperature sintering to obtain LATP / Ni@Co@Mo catalyst: The mixture of LATP precursor and Ni@Co@Mo catalyst was placed in an atmosphere furnace, nitrogen was introduced at a flow rate of 1m³ / h, the temperature was increased to 800°C at a heating rate of 2.5°C / min, kept warm for 4h, then increased to 1100°C at a heating rate of 2°C / min, kept warm for 6h, and naturally cooled to room temperature to obtain LATP / Ni@Co@Mo catalyst.

[0096] 4) Preparation of composite lithium supplement: The lithium oxalate was evenly dispersed in deionized water, the mass ratio of lithium oxalate to deionized water was 1:7, and then transferred to a sand mill and ground at 2000rpm for 3h to obtain nano-Li2C2O4. The LATP / Ni@Co@Mo catalyst and nano-Li2C2O4 were evenly dispersed in deionized water at a mass ratio of 1:5, and ultrasonically treated at 2500 W for 1h. Then, the mixed solution was transferred to a polytetrafluoroethylene-lined pressure reactor and hydrothermally reacted at 200°C for 8h to obtain a composite lithium supplement of LATP / Ni@Co@Mo catalyst-coated nano-lithium oxalate.

[0097] Example 4 1) Preparation of Ni@Co@Mo metal aerogel: Same as step 1 of Example 1).

[0098] 2) Preparation of Ni@Co@Mo aerogel with LLZO precursor filled in the pores: Weigh 480g of LiNO3, 1300g of La(NO3)3·6H2O, 650g of ZrC2H3O2)4 and 800g of citric acid, then dissolve them in 5L of deionized water, stir at 45°C and 250 rpm for 120 min to obtain a uniformly mixed LLZO precursor solution; pour the LLZO precursor solution into the Ni@Co@Mo aerogel (the mass ratio of the LLZO precursor solution to the Ni@Co@Mo aerogel is 20:1), fill the LLZO precursor solution into the pores of the Ni@Co@Mo aerogel, and dry at 50°C for 36h to obtain a Ni@Co@Mo metal aerogel with pores filled with LLZO precursor.

[0099] 3) High temperature sintering to obtain LLZO / Ni@Co@Mo aerogel: The Ni@Co@Mo metal aerogel with LLZO precursor in the pores was placed in an atmosphere furnace, nitrogen was introduced at a flow rate of 1m³ / h, the temperature was increased to 950°C at a heating rate of 0.5°C / min, and the temperature was kept for 12h. After naturally cooling to room temperature, LLZO / Ni@Co@Mo aerogel was obtained.

[0100] 4) Preparation of composite lithium supplement: The lithium oxalate was evenly dispersed in deionized water at a mass ratio of 1:10, and then transferred to a sand mill and ground at 500rpm for 8h to obtain nano-Li2C2O4. The LLZO / Ni@Co@Mo aerogel and the nano-Li2C2O4 were evenly dispersed in deionized water at a mass ratio of 1:9, and ultrasonically treated at 3000 W for 0.5h. Then, the mixed solution was transferred to a polytetrafluoroethylene-lined pressure reactor and hydrothermally reacted at 140°C for 24h to obtain a composite lithium supplement of LLZO / Ni@Co@Mo aerogel-coated nano-lithium oxalate.

[0101] Example 5 1) Preparation of Ni@Co@Mo metal aerogel: Same as step 1) of Example 3).

[0102] 2) Preparation of Ni@Co@Mo aerogel with pores filled with LLTO precursor: Weigh 25 g of LiNO3, 240 g of La(NO3)3·6H2O, 1000 g of Ti(OC4H9)4 and 640 g of citric acid, then dissolve them in 5 L of deionized water, and stir them at 60°C and 200 rpm for 90 min to obtain a uniformly mixed LLTO precursor solution; pour the LLTO precursor solution into the Ni@Co@Mo aerogel (the mass ratio of the LLTO precursor solution to the Ni@Co@Mo aerogel is 15:1), so that the LLTO precursor solution fills the pores of the Ni@Co@Mo aerogel, and dry them at 60°C for 36 h to obtain a Ni@Co@Mo metal aerogel with pores filled with LLTO precursor.

[0103] 3) High temperature sintering to obtain LLTO / Ni@Co@Mo aerogel: The Ni@Co@Mo metal aerogel with LLTO precursor in the pores was placed in an atmosphere furnace, nitrogen was introduced at a flow rate of 0.5 m³ / h, the temperature was increased to 600°C at a heating rate of 0.5°C / min, and the temperature was kept for 5 h. Then the temperature was increased to 1100°C at a heating rate of 1°C / min, and the temperature was kept for 12 h. After naturally cooling to room temperature, LLTO / Ni@Co@Mo aerogel was obtained.

[0104] 4) Preparation of composite lithium supplement: The lithium oxalate was evenly dispersed in deionized water at a mass ratio of 1:10, and then transferred to a sand mill and ground at 500rpm for 8h to obtain nano-Li2C2O4. The LLTO / Ni@Co@Mo aerogel and the nano-Li2C2O4 were evenly dispersed in deionized water at a mass ratio of 1:9, and ultrasonically treated at 3000 W for 0.5h. Then, the mixed solution was transferred to a polytetrafluoroethylene-lined pressure reactor and hydrothermally reacted at 140°C for 24h to obtain a composite lithium supplement of LLTO / Ni@Co@Mo aerogel-coated nano-lithium oxalate.

[0105] Preparation of button cells: The composite lithium supplement prepared in Examples 1 to 5 and Comparative Examples 1 to 4 was used as the positive electrode active material, the conductive agent SP, and the binder PVDF were mixed in a mass ratio of 85:10:5, and then mixed with a solvent N-methylpyrrolidone (NMP). The obtained mixed slurry (solid content of 25%) was coated (coating thickness of 250 μm) on an aluminum foil, and then placed in a 120°C blast oven for drying for 12 h, and then rolled and punched to make a positive electrode sheet; a metal lithium sheet was used as a negative electrode, a celgard2400 polypropylene porous membrane was used as a diaphragm, and a 1 mol / L LiPF6 solution (the solvent was ethylene carbonate (EC) and dimethyl carbonate (DMC), and the volume ratio was 1:1) as an electrolyte; the process was carried out in a glove box filled with argon gas, the water oxygen value in the glove box was controlled to be less than 0.01 ppm, and the battery was pressurized and sealed with a sealing machine to obtain a button battery.

[0106] The button cell was subjected to electrochemical performance testing to test the delithiation potential and initial charge and discharge specific capacity of the lithium supplement material. The reduction in the delithiation potential of the lithium supplement material can effectively alleviate the interfacial side reactions between the positive electrode material and the electrolyte at high desorption potential. The initial charge and discharge specific capacity also reflects the amount of active lithium provided by the lithium supplement material in the battery system. The battery test was carried out at a constant temperature of 25°C, and the charge and discharge mode was: 0.1C constant current charging, 0.1C constant current discharging. The test results are shown in Table 1.

[0107] Table 1 Electrochemical performance data of button cells Under the same battery system, compared with battery No. 6, the delithiation potential of battery No. 1 is significantly lower than that of battery No. 6, indicating that the metal aerogel catalyst filled with LATP solid electrolyte can significantly reduce the delithiation potential of lithium oxalate. A large number of active sites and high specific surface area can improve the catalytic effect and accelerate the catalytic reaction. Compared with battery No. 9, the lithium oxalate supplement coated with LATP / Ni@Co@Mo aerogel in batteries No. 3~5 can provide more active lithium to compensate for the negative effects such as capacity reduction caused by the loss of active lithium due to SEI film formation. Compared with battery No. 7, the lithium oxalate coated with LATP / Ni@Co@Mo aerogel in battery No. 1 has better ionic conductivity, reduces the energy barrier of lithium ion deintercalation, has a lower delithiation potential and a higher first discharge specific capacity. Compared with No. 8 battery, No. 2 battery uses lithium oxalate coated with LATP / Ni@Co@Mo aerogel. Ni@Co@Mo aerogel has more metal catalytic sites and a larger specific surface area, which can greatly improve the conductivity of lithium oxalate, reduce the decomposition energy barrier, and have a lower separation potential.

[0108] Preparation of soft pack batteries: Using single crystal morphology LiNi 0.92 Co0.055 Mn 0.25 O2, a PVDF solution with a mass concentration of 1.5% (the solvent is NMP), a conductive agent Super P and a composite lithium supplement (the composite lithium supplements prepared in Examples 1 to 5 and Comparative Examples 1 to 4, respectively) were mixed in a mass ratio of 94:3:1.5:1.5, and NMP was added to obtain a positive electrode slurry with a solid content of 50%; the obtained positive electrode slurry was coated (the coating speed was 1 m / min, and the single-sided coating thickness was 246 μm) on both sides of a 20 μm aluminum foil, and dried at 145°C to obtain a positive electrode sheet.

[0109] The negative electrode material silicon carbon negative electrode 1800 (Cruder), conductive agent Super P, thickener (deionized water solution of sodium carboxymethyl cellulose CMC, mass concentration of 1.5%), binder (deionized water solution of styrene-butadiene rubber SBR, mass concentration of 48%), deionized water solution of polyacrylic acid PAA (mass concentration of 6%), and deionized water solution of single-walled carbon nanotube CNT (mass concentration of 0.4%) were mixed at a mass ratio of 95:0.9:1:1:2:0.1. After mixing, deionized water was added to control the theoretical solid content to 35%. The negative electrode slurry was obtained by homogenization using a vacuum defoamer, and the negative electrode slurry was evenly coated on a copper foil with a thickness of 17 μm. After drying, rolling and cutting, a 52 mm×72 mm negative electrode sheet was obtained. The N / P ratio of the positive and negative electrodes is 1.1.

[0110] The positive electrode sheet and the negative electrode sheet are respectively rolled and the tabs are welded to prepare a soft-pack battery.

[0111] The soft-pack battery was subjected to an electrochemical performance test. The design voltage of the soft-pack battery was 3-4.25 V, and the design capacity was 2.5 Ah.

[0112] Test standard: The soft-pack batteries were tested for room temperature cycle performance, and the results are shown in Table 2.

[0113] Battery room temperature cycle performance test: The prepared soft-pack battery was placed in a constant temperature room with an ambient temperature of 25°C, charged at a constant current of 1C to a voltage of 4.25V, then charged at a constant voltage of 4.25V to a current of 0.05C, and then discharged at a constant current of 1C to a voltage of 3.0V. The cycle was repeated for 2000 times, and the capacity retention rate was recorded. The capacity retention rate of the nth cycle (%) = (discharge capacity of the nth cycle / discharge capacity of the first cycle) × 100%.

[0114] Table 2 Electrochemical performance data of soft pack batteries As can be seen from Table 2, under the same battery system, the average 1C capacity of batteries No. 10 to No. 14 at room temperature is greater than 2.49 Ah; after 2000 cycles, batteries No. 10 to No. 14 show good cycle stability, and the 2000-week cycle retention rate is greater than 96.3%. This is because as the cycle progresses, the SEI on the surface of the positive and negative electrode materials will expand in volume, and the electrolyte and the surface of the positive and negative electrode materials will undergo interfacial side reactions, causing destruction and reconstruction. In this process, a new SEI is re-formed, and a part of the active lithium will be lost. The use of composite lithium oxalate lithium supplement can provide it with a large amount of active lithium, so the 2000-week cycle retention rate is relatively high.

[0115] Compared with No. 15 battery, the 1C capacity and 2000-cycle retention rate of No. 12 battery are significantly increased. This is because the lithium oxalate supplement is coated with LATP solid electrolyte. After the decomposition of lithium oxalate, LATP solid electrolyte has a good ion channel, which can greatly slow down the energy barrier of lithium ion deintercalation and reduce internal energy loss. Compared with No. 17~18 batteries, No. 10 battery has a higher 1C capacity and excellent 2000-cycle retention, because the lithium oxalate deintercalation potential of No. 10 battery is lower than 4.2V, while the lithium oxalate used in No. 17~18 battery is difficult to decompose at a voltage of 4.2V and cannot release active lithium. It shows that the innovative technology of LATP / Ni@Co@Mo aerogel coating not only improves the structural stability of lithium oxalate, but also promotes its decomposition and release of active lithium during the battery charging and discharging process. The addition of LATP improves the ionic conductivity of the material, while the multi-metal synergistic effect of Ni@Co@Mo optimizes the electrochemical reaction kinetics, further reduces the delithiation potential, and makes the release of active lithium smoother.

[0116] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.

Claims

1. A composite comprising a metal aerogel and a solid electrolyte; The metal aerogel is Ni@Co@M metal aerogel, where M is Mo or Fe; The solid electrolyte is selected from lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide or lithium lanthanum titanium oxide.

2. The composite according to claim 1, characterized in that The composite is obtained by sintering a mixture of a solid electrolyte precursor solution and a metal aerogel at high temperature.

3. The composite according to claim 2, characterized in that The preparation method of the mixture comprises the following steps: The solid electrolyte precursor solution is mixed with the metal aerogel and dried to obtain a mixture.

4. The composite according to claim 2, characterized in that The high temperature sintering comprises: The mixture is heated to 700-900° C. and kept warm, and then heated to 1000-1200° C. and kept warm; The high-temperature sintering is performed under a protective gas atmosphere.

5. The composite according to claim 4, characterized in that The heating rate to 700-900°C is 0.5-5°C / min, and the holding time at 700-900°C is 3-6 h; The heating rate for reheating to 1000~1200℃ is 1~4℃ / min, and the holding time at 1000~1200℃ is 5~10 h.

6. The composite according to claim 1, characterized in that The preparation method of the Ni@Co@M metal aerogel comprises the following steps: An aqueous solution containing a structure directing agent and a complexing agent, a cobalt source, a nickel source, an M source and a reducing agent are mixed, deoxygenated, heated and stirred at 40-80° C. to form a hydrogel, and dried or solvent replaced to obtain a Ni@Co@M metal aerogel; the M source is a Mo source or a Fe source.

7. The composite according to claim 6, characterized in that The structure directing agent comprises at least one of a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, hexadecyltrimethylammonium bromide and a polyoxyethylene polyoxypropylene ether block copolymer; The complexing agent includes at least one of sodium citrate, nitrilotriacetic acid, ethylenediaminetetraacetic acid and adenosine triphosphate; The mass ratio of the structure directing agent to the complexing agent is (40-80): (60-120); In the aqueous solution containing the structure directing agent and the complexing agent, the mass ratio of the total mass of the structure directing agent and the complexing agent to water is 1:(15-25).

8. The composite according to claim 6, characterized in that The cobalt source includes at least one of cobalt acetate, cobalt acetylacetonate and cobalt nitrate; The nickel source includes nickel acetate and / or nickel nitrate; The Mo source includes molybdenum acetate dimer and / or ammonium molybdate; The Fe source includes ferric nitrate and / or ferric acetylacetonate; The reducing agent includes at least one of dimethylamine borane, sodium borohydride, ascorbic acid and metal organic framework MOFs.

9. The composite according to claim 6, characterized in that The mass ratio of the structure directing agent, the complexing agent, the cobalt salt, the nickel salt, the M source and the reducing agent is (40-80):(60-120):(100-150):(100-150):(100-150):(800-1000).

10. A composite lithium supplement, characterized in that: include: Lithium oxalate; An aerogel coating layer formed on the surface of the lithium oxalate; The component of the aerogel coating layer is the composite material according to any one of claims 1 to 9.

11. The method for preparing the composite lithium supplement according to claim 10, comprising the following steps: A) Grinding the aqueous solution of lithium oxalate to obtain nano-Li2C2O4; B) The composite and the nano-Li2C2O4 are uniformly dispersed in deionized water, and after ultrasonic treatment, a hydrothermal reaction is performed to obtain a composite lithium supplement.

12. The preparation method according to claim 11, characterized in that: In step B), the mass ratio of the composite to the nano-Li2C2O4 is 1:(3-9); The power of the ultrasonic treatment is 500-3000 W, and the time is 0.5-5 h; The temperature of the hydrothermal reaction is 140-220° C., and the time is 6-24 h.

13. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery includes a composite lithium supplement; The composite lithium supplement is the composite lithium supplement according to claim 10, or is the composite lithium supplement obtained by the preparation method according to any one of claims 11 to 12.

Citation Information

Patent Citations

  • Composite solid electrolyte based on inorganic ceramic three-dimensional aerogel skeleton support and preparation method thereof

    CN113270634A

  • Lithium supplement agent for positive electrode material of lithium battery and preparation method of lithium supplement agent

    CN115275200A

  • Lithium supplement composite material and preparation method and application thereof

    CN117559013A

  • Lithium-rich positive electrode material and preparation method and application thereof

    CN117712320A

  • Positive electrode composite material, preparation method thereof and lithium ion battery

    CN117766705A

Cited By

  • Lithium ferrite lithium supplement agent and preparation method and application thereof

    CN119447310A

  • Preparation method and application of aqueous nano-composite lithium-supplementing diaphragm

    CN119965458A

  • ZIF-67-derived composite lithium oxalate lithium supplement agent as well as preparation method and application thereof

    CN121662996A

  • A zif-67 derived composite lithium oxalate lithium supplementing agent, a preparation method and application thereof

    CN121662996B

  • Composite lithium supplement agent and preparation method thereof, positive pole piece and lithium ion battery

    CN122246320A