Synthesis method of morphology-adjustable transition metal phosphide Pt-based composite catalyst
By regulating the morphological structure of the transition metal phosphide Pt-based catalyst, a hydrangea, spherical and sheet-like Pt/Fe2P-CoP-NDC composite catalyst is formed, which solves the problem of regulating the catalyst morphological structure in the prior art and significantly improves the Catalytic activity and stability have promoted the commercialization process of DMFC.
Patent Information
- Application Number
- CN202411151622.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The prior art is difficult to accurately regulate the morphological structure of transition metal phosphide Pt-based catalysts, resulting in a reduction in catalytic activity and stability, limiting the large-scale commercial application of direct methanol fuel cells (DMFCs).
Fe2P-CoP-NDC composite carrier was prepared by preparing the precursors Fe-DCD and Fe-Co-DCD, combining surfactant and triphenylphosphine, and calcining at specific temperatures and atmospheres, and loading Pt nanoparticles by acid etching. A hydrangea, spherical and sheet-like Pt/Fe2P-CoP-NDC composite catalyst is formed to regulate its morphological structure.
The specific surface area and pore structure of the catalyst are improved, the interaction force between Pt NPs and the support material is enhanced, the Pt particle size, dispersion and anti-CO poisoning ability are optimized, and the catalytic activity and stability are significantly improved.
Smart Images

Figure CN119050379A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrocatalysis, and in particular relates to a method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology. Background Art
[0002] As an energy conversion device, direct methanol fuel cell (DMFC) has been widely studied due to its high energy conversion efficiency, abundant fuel sources, easy storage and low pollution emissions. At present, the lack of efficient catalysts for DMFC anode is one of the main reasons restricting its large-scale commercial application. A large number of studies have shown that precious metal Pt is still the best choice for catalytic oxidation of methanol. However, Pt is expensive and easily poisoned by the intermediate product CO. Therefore, achieving small-size dispersion of Pt nanoparticles and improving the utilization rate of precious metal Pt are of great significance to reducing costs and improving the methanol oxidation activity of Pt-based composite catalysts.
[0003] Transition metal phosphides have attracted extensive attention due to their excellent catalytic effect. δ+ and P δ- Active sites can play a significant promoting role, activating water molecules at a lower potential, accelerating the decomposition of H2O, producing abundant hydroxyl components to participate in the reaction, and removing CO-like intermediates chemically adsorbed on the active sites of Pt nanoparticles, thereby releasing more active sites to participate in the reaction and increasing the utilization rate of precious metals. At the same time, based on the bifunctional mechanism and electronic effect, the embedding of transition metal phosphides can greatly improve the methanol oxidation activity of the catalyst. However, transition metal phosphides have poor stability and mostly exist in the form of particles. They inevitably aggregate and dissolve during the electrocatalytic process, resulting in the burial of the active sites of the catalyst and reduced catalytic activity and stability. Therefore, precise control of its morphology and structure has an important influence on optimizing the size, dispersion, and surface state of Pt nanoparticles.
[0004] Up to now, there are few reports on the precise control of the morphology and structure of Pt-based catalysts based on transition metal phosphides. Therefore, screening and constructing inexpensive, readily available, and excellent electrocatalytic materials are of great significance to promoting the large-scale commercialization of DMFCs. Generally, large specific surface area and suitable pore structure can promote mass transfer and electron transfer during the reaction process, and accelerate the reaction kinetics and reaction process of methanol oxidation. At the same time, regulating the morphology and structure of the catalyst can not only effectively enhance the interaction between PtNPs and the support material, and improve the catalytic stability of Pt-based catalysts in methanol oxidation reactions, but also the morphology and structure play a key role in optimizing the size, dispersion, surface state, exposed crystal surface, number of active sites, and resistance to CO poisoning of Pt particles, thereby affecting the catalytic activity of Pt-based catalysts. Therefore, designing, constructing, and controlling the morphology and structure of Pt-based catalysts is of great reference significance for improving catalytic performance and exploring the reaction mechanism during methanol oxidation reactions. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for synthesizing a transition metal phosphide Pt-based composite catalyst with controllable morphology.
[0006] The purpose of the present invention is achieved by the following technical scheme: a method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology, which comprises the following steps:
[0007] S1. Preparation of Fe-DCD precursor: Dissolve ferric nitrate and dicyandiamide in ethanol solution, heat in a water bath to 70-90°C, and continue stirring until ethanol is completely evaporated to obtain Fe-DCD precursor;
[0008] S2. Preparation of Fe-Co-DCD precursor: The precursor Fe-DCD, surfactant and cobalt nitrate prepared in step S1 are dissolved in methanol to obtain solution A; the methanol solution of dimethylimidazole is slowly added to solution A and mixed evenly, and then transferred to a reactor and reacted at 110-130° C. for 10-14 hours to generate a Fe-Co-DCD precursor;
[0009] S3. Preparation of composite support: After the Fe-Co-DCD precursor and triphenylphosphine were mixed and ground evenly, they were calcined at 580-620 ° C for 1.5-2.5 h in a nitrogen atmosphere, and then calcined at 780-820 ° C for 1.5-2.5 h to obtain a Fe2P-CoP-NDC composite support;
[0010] S4. Preparation of composite catalyst: The Fe2P-CoP-NDC composite carrier obtained in step S3 is acid-etched, and Pt nanoparticles are loaded after acid etching to obtain a Pt / Fe2P-CoP-NDC composite catalyst.
[0011] As a preferred technical solution, the weight ratio of ferric nitrate to dicyandiamide in step S1 is 1:3-5, and the volume ratio of the total mass of ferric nitrate and dicyandiamide to the ethanol solution is 1g:20-30ml.
[0012] As a preferred technical solution, the surfactant in step S2 is any one of cetyltrimethylammonium bromide, polyvinylpyrrolidone or sodium dodecylbenzenesulfonate. If the surfactants are cetyltrimethylammonium bromide, polyvinylpyrrolidone and sodium dodecylbenzenesulfonate respectively, the morphologies of the prepared Pt / Fe2P-CoP-NDC composite catalyst are hydrangea-shaped, spherical and lamellar respectively.
[0013] As a preferred technical solution, the weight ratio of the precursor Fe-DCD, surfactant and cobalt nitrate in step S2 is 1:1.5~3:1.2~1.8, the mass volume ratio of dimethylimidazole to methanol solution in the methanol solution of dimethylimidazole is 0.2~0.4g:10ml; the volume ratio of solution A to the methanol solution of dimethylimidazole is 1.5~3:1.
[0014] As a preferred technical solution, the weight ratio of triphenylphosphine to Fe-DCD in step S3 is 3 to 5:1.
[0015] As a preferred technical solution, the heating rate in step S3 is 1.5-2.5°C / min.
[0016] As a preferred technical solution, the specific operation of the acid etching in step S4 is: the Fe2P-CoP-NDC composite carrier is immersed in a 0.3-0.8M H2SO4 solution for acid etching for 50-70 minutes.
[0017] As a preferred technical solution, the specific operation steps of loading Pt nanoparticles in step S4 are:
[0018] S41. The Fe2P-CoP-NDC composite carrier is dispersed in deionized water and uniformly dispersed by ultrasonication, which is recorded as solution B. The concentration of the Fe2P-CoP-NDC composite carrier in solution B is 0.8-1.2 mg / ml; trisodium citrate and 48.803 mM H2PtCl6-EG (ethylene glycol solution of chloroplatinic acid) are dissolved in deionized water, which is recorded as solution C. The concentration of trisodium citrate in solution C is 4-6 mg / ml, and the volume ratio of H2PtCl6-EG to deionized water is 1:8-12; NaBH4 is dissolved in deionized water, which is recorded as solution D. The concentration of NaBH4 in solution D is 0.3-0.7 mg / ml;
[0019] S42. While stirring at a speed of 400 to 700 r / min, slowly add solution C to solution B. After mixing evenly, add solution D dropwise. The volume ratio of solution B, solution C and solution D is 3 to 5:1:1.2 to 2. Continue stirring at room temperature for 22 to 26 hours. After the reaction is completed, filter and wash with anhydrous ethanol and deionized water. Then, dry at a temperature of 55 to 65°C for 10 to 14 hours to obtain a transition metal phosphide Pt-based composite catalyst.
[0020] The present invention has the following advantages: The present invention discloses a method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology, and the method of the present invention can obtain hydrangea-shaped, spherical and lamellar Pt / Fe2P-CoP-NDC composite catalysts. Compared with the existing granular transition metal phosphide Pt-based composite catalysts, the present invention increases the specific surface area and improves the pore structure, and can accelerate the reaction kinetics and reaction process of methanol oxidation. At the same time, by regulating the morphology, the interaction between Pt NPs and the carrier material can be effectively enhanced, the catalytic stability of the Pt-based catalyst in the methanol oxidation reaction can be improved, and it plays a key role in optimizing the Pt particle size, dispersion, surface state, exposed crystal surface, number of active sites and CO poisoning resistance, thereby improving the catalytic activity of the Pt-based catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 XRD patterns of hydrangea-shaped Pt / Fe2P-CoP-NDC (h), spherical Pt / Fe2P-CoP-NDC (s) and lamellar Pt / Fe2P-CoP-NDC (f) composite catalysts.
[0022] Figure 2 This is the SEM image of the lamellar Pt / Fe2P-CoP-NDC catalyst.
[0023] Figure 3 This is the SEM image of the hydrangea-shaped Pt / Fe2P-CoP-NDC catalyst.
[0024] Figure 4 SEM image of spherical Pt / Fe2P-CoP-NDC catalyst.
[0025] Figure 5 CV curves of hydrangea-shaped Pt / Fe2P-CoP-NDC (h), spherical Pt / Fe2P-CoP-NDC (s) and lamellar Pt / Fe2P-CoP-NDC (f) composite catalysts.
[0026] Figure 6Mass activity diagrams of hydrangea-shaped Pt / Fe2P-CoP-NDC (h), spherical Pt / Fe2P-CoP-NDC (s) and lamellar Pt / Fe2P-CoP-NDC (f) composite catalysts.
[0027] Figure 7 The specific activity diagram of hydrangea-shaped Pt / Fe2P-CoP-NDC (h), spherical Pt / Fe2P-CoP-NDC (s) and lamellar Pt / Fe2P-CoP-NDC (f) composite catalysts.
[0028] Figure 8 CA curves of hydrangea-shaped Pt / Fe2P-CoP-NDC (h), spherical Pt / Fe2P-CoP-NDC (s) and lamellar Pt / Fe2P-CoP-NDC (f) composite catalysts.
[0029] Fig. 9 This is a comparison chart of the mass activity of the layered Pt / Fe2P-CoP-NDC(f) catalyst before and after 1000 cycles of testing.
[0030] Fig.10 This is a comparison chart of the mass activity of the hydrangea-shaped Pt / Fe2P-CoP-NDC(h) catalyst before and after 1000 cycles of testing.
[0031] Fig.11 This is a comparison chart of the mass activity of spherical Pt / Fe2P-CoP-NDC(s) catalyst before and after 1000 cycles of testing. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with the accompanying drawings and embodiments, and the protection scope of the present invention is not limited to the following: Embodiment 1: A method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology, comprising the following steps: S1. Preparing a precursor Fe-DCD: dissolving ferric nitrate and dicyandiamide in an ethanol solution, heating and keeping warm in a water bath to 70°C, and continuously stirring until the ethanol is completely evaporated to obtain a precursor Fe-DCD; wherein the weight ratio of the ferric nitrate to dicyandiamide is 1:3, and the volume ratio of the total mass of the ferric nitrate and dicyandiamide to the ethanol solution is 1g:20ml;
[0033] S2. Preparation of Fe-Co-DCD precursor: The precursor Fe-DCD, hexadecyltrimethylammonium bromide and cobalt nitrate prepared in step S1 are dissolved in methanol to obtain solution A; the methanol solution of dimethylimidazole is slowly added to solution A and mixed evenly, and then transferred to a reactor and reacted at 110° C. for 10 h to generate a Fe-Co-DCD precursor;
[0034] The weight ratio of the precursor Fe-DCD, the surfactant and the cobalt nitrate is 1:1.5:1.2, the mass volume ratio of dimethylimidazole to the methanol solution in the dimethylimidazole methanol solution is 0.2g:10ml; the volume ratio of the solution A to the dimethylimidazole methanol solution is 1.5:1;
[0035] S3. Preparation of composite carrier: After the Fe-Co-DCD precursor and triphenylphosphine were mixed and ground evenly, the weight ratio of triphenylphosphine to Fe-DCD was 3:1, and the temperature was increased to 580°C at a rate of 1.5°C / min under a nitrogen atmosphere and calcined for 1.5h, and then the temperature was increased to 780°C at a rate of 1.5°C / min and calcined for 1.5h to obtain a hydrangea-shaped Fe2P-CoP-NDC composite carrier;
[0036] S4. Preparation of composite catalyst: The hydrangea-shaped Fe2P-CoP-NDC composite carrier obtained in step S3 was immersed in a 0.3M H2SO4 solution and acid-etched for 50 min, and the Pt nanoparticles were loaded after acid etching. The specific operation steps of the loaded Pt nanoparticles are as follows:
[0037] S41. The hydrangea-shaped Fe2P-CoP-NDC composite carrier was dispersed in deionized water and uniformly dispersed by ultrasonication, which was recorded as solution B. The concentration of the Fe2P-CoP-NDC composite carrier in solution B was 0.8 mg / ml; trisodium citrate and 48.803 mM H2PtCl6-EG (ethylene glycol solution of chloroplatinic acid) were dissolved in deionized water, which was recorded as solution C. The concentration of trisodium citrate in solution C was 4 mg / ml, and the volume ratio of H2PtCl6-EG to deionized water was 1:8; NaBH4 was dissolved in deionized water, which was recorded as solution D. The concentration of NaBH4 in solution D was 0.3 mg / ml;
[0038] S42. While stirring at a speed of 400 r / min, solution C was slowly added to solution B. After mixing evenly, solution D was added dropwise. The volume ratio of solution B, solution C and solution D was 3:1:1.2. Stirring was continued at room temperature for 22 hours. After the reaction was completed, the mixture was filtered and washed with anhydrous ethanol and deionized water. It was then dried at 55°C for 10 hours to obtain a hydrangea-shaped transition metal phosphide Pt-based composite catalyst.
[0039] Embodiment 2: A method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology, comprising the following steps: S1. Preparing a precursor Fe-DCD: dissolving ferric nitrate and dicyandiamide in an ethanol solution, heating the solution in a water bath to 90°C, and continuously stirring the solution until the ethanol is completely evaporated, to obtain a precursor Fe-DCD; wherein the weight ratio of the ferric nitrate to dicyandiamide is 1:5, and the volume ratio of the total mass of the ferric nitrate and dicyandiamide to the ethanol solution is 1g:30ml;
[0040] S2. Preparation of Fe-Co-DCD precursor: The precursor Fe-DCD, polyvinyl pyrrolidone and cobalt nitrate prepared in step S1 are dissolved in methanol to obtain solution A; the methanol solution of dimethylimidazole is slowly added to solution A and mixed evenly, and then transferred to a reactor and reacted at 130° C. for 14 hours to generate a Fe-Co-DCD precursor;
[0041] The weight ratio of the precursor Fe-DCD, the surfactant and the cobalt nitrate is 1:3:1.8, the mass volume ratio of dimethylimidazole to the methanol solution in the dimethylimidazole methanol solution is 0.4g:10ml; the volume ratio of the solution A to the dimethylimidazole methanol solution is 3:1;
[0042] S3. Preparation of composite support: After the Fe-Co-DCD precursor and triphenylphosphine were mixed and ground evenly, the weight ratio of triphenylphosphine to Fe-DCD was 5:1, and the temperature was increased to 620°C at a rate of 2.5°C / min under a nitrogen atmosphere and calcined for 2.5h, and then the temperature was increased to 820°C at a rate of 2.5°C / min and calcined for 2.5h to obtain a spherical Fe2P-CoP-NDC composite support;
[0043] S4. Preparation of composite catalyst: The spherical Fe2P-CoP-NDC composite carrier obtained in step S3 was immersed in a 0.8MH2SO4 solution and acid-etched for 70 min, and the loaded Pt nanoparticles were loaded after acid etching. The specific operation steps of the loaded Pt nanoparticles are as follows:
[0044] S41. The spherical Fe2P-CoP-NDC composite carrier was dispersed in deionized water and uniformly dispersed by ultrasonication, which was recorded as solution B. The concentration of the Fe2P-CoP-NDC composite carrier in solution B was 1.2 mg / ml; trisodium citrate and 48.803 mM H2PtCl6-EG (ethylene glycol solution of chloroplatinic acid) were dissolved in deionized water, which was recorded as solution C. The concentration of trisodium citrate in solution C was 6 mg / ml, and the volume ratio of H2PtCl6-EG to deionized water was 1:12; NaBH4 was dissolved in deionized water, which was recorded as solution D. The concentration of NaBH4 in solution D was 0.7 mg / ml;
[0045] S42. While stirring at a speed of 700 r / min, solution C is slowly added to solution B. After mixing evenly, solution D is added dropwise. The volume ratio of solution B, solution C and solution D is 5:1:2. Stirring is continued at room temperature for 26 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol and deionized water. Then, it is dried at 65°C for 14 hours to obtain a spherical transition metal phosphide Pt-based composite catalyst.
[0046] Embodiment 3: A method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology, comprising the following steps: S1. Preparing a precursor Fe-DCD: dissolving ferric nitrate and dicyandiamide in an ethanol solution, heating the solution in a water bath to 80°C, and continuously stirring the solution until the ethanol is completely evaporated, to obtain a precursor Fe-DCD; wherein the weight ratio of the ferric nitrate to dicyandiamide is 1:4, and the volume ratio of the total mass of the ferric nitrate and dicyandiamide to the ethanol solution is 1g:25ml;
[0047] S2. Preparation of Fe-Co-DCD precursor: The precursor Fe-DCD, sodium dodecylbenzene sulfonate and cobalt nitrate prepared in step S1 are dissolved in methanol to obtain solution A; the methanol solution of dimethylimidazole is slowly added to solution A and mixed evenly, and then transferred to a reactor and reacted at 120° C. for 12 hours to generate a Fe-Co-DCD precursor;
[0048] The weight ratio of the precursor Fe-DCD, the surfactant and the cobalt nitrate is 1:2:1.5, the mass volume ratio of dimethylimidazole to the methanol solution in the dimethylimidazole methanol solution is 0.3g:10ml; the volume ratio of the solution A to the dimethylimidazole methanol solution is 2:1;
[0049] S3. Preparation of composite support: After the Fe-Co-DCD precursor and triphenylphosphine were mixed and ground evenly, the weight ratio of triphenylphosphine to Fe-DCD was 4:1, and the temperature was increased to 600 ° C for 2 h at a heating rate of 2 ° C / min under a nitrogen atmosphere, and then the temperature was increased to 800 ° C for 2 h at a heating rate of 2 ° C / min to obtain a lamellar Fe2P-CoP-NDC composite support;
[0050] S4. Preparation of composite catalyst: The lamellar Fe2P-CoP-NDC composite carrier obtained in step S3 was immersed in a 0.5MH2SO4 solution for 60 min, and the Pt nanoparticles were loaded after acid etching. The specific operation steps of the loaded Pt nanoparticles are as follows:
[0051] S41. The lamellar Fe2P-CoP-NDC composite carrier is dispersed in deionized water and uniformly dispersed by ultrasonication, which is referred to as solution B. The concentration of the Fe2P-CoP-NDC composite carrier in solution B is 1 mg / ml; trisodium citrate and 48.803 mM H2PtCl6-EG (ethylene glycol solution of chloroplatinic acid) are dissolved in deionized water, which is referred to as solution C. The concentration of trisodium citrate in solution C is 5 mg / ml, and the volume ratio of H2PtCl6-EG to deionized water is 1:10; NaBH4 is dissolved in deionized water, which is referred to as solution D. The concentration of NaBH4 in solution D is 0.5 mg / ml;
[0052] S42. While stirring at a speed of 500 r / min, slowly add solution C into solution B. After mixing evenly, add solution D dropwise. The volume ratio of solution B, solution C and solution D is 4:1:1.5. Continue stirring at room temperature for 24 hours. After the reaction is completed, filter and wash with anhydrous ethanol and deionized water, and then dry at 60°C for 12 hours to obtain a lamellar transition metal phosphide Pt-based composite catalyst.
[0053] The beneficial effects of the present invention are described below by experiments:
[0054] Example 1: A method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology, comprising the following steps: S1. Preparing a precursor Fe-DCD: 0.404 g of ferric nitrate and 1.68 g of dicyandiamide are dissolved in 50 mL of ethanol solution, heated in a water bath to 80° C., and stirred continuously until the ethanol is completely evaporated, to obtain a precursor Fe-DCD;
[0055] S2. Preparation of Fe-Co-DCD precursor: 0.2 g of the precursor prepared in step S1 Fe-DCD, 0.4g hexadecyltrimethylammonium bromide and 0.3g cobalt nitrate were dissolved in 20mL methanol to obtain solution A; 0.3g dimethylimidazole was dissolved in 10mL methanol, slowly added to solution A and mixed evenly, then transferred to a 50mL reactor and reacted at 120°C for 12h, cooled to room temperature, filtered, washed several times with anhydrous ethanol and deionized water, and dried in a 60°C oven for 12h to generate a Fe-Co-DCD precursor; S3. Preparation of composite carrier: Use a quartz mortar to mix and grind the dried Fe-Co-DCD precursor and 0.7g triphenylphosphine evenly, transfer to a porcelain boat, and place it in the middle of a tube furnace, and heat it to 600°C at a rate of 2°C / min in a nitrogen atmosphere for calcination for 2h, and then heat it to 800°C at a rate of 2°C / min for calcination for 2h to obtain a Fe2P-CoP-NDC composite carrier;
[0056] S4. Preparation of composite catalyst: The Fe2P-CoP-NDC composite carrier was immersed in a 0.5M H2SO4 solution and acid-etched for 60 min, and Pt nanoparticles were loaded after acid etching. The specific operation steps of the loaded Pt nanoparticles were as follows:
[0057] S41. Accurately weigh 0.02g of Fe2P-CoP-NDC composite carrier, disperse it in 20mL of deionized water, and ultrasonically disperse it for 20min to make it uniform, which is recorded as solution B; 0.0245g of trisodium citrate and 0.525mL48.803 mM H2PtCl6-EG (ethylene glycol solution of chloroplatinic acid) are dissolved in 5mL of deionized water, which is recorded as solution C; 4.6mgNaBH4 is dissolved in 8mL of deionized water, which is recorded as solution D;
[0058] S42. While stirring at a speed of 500 r / min, slowly add solution C into solution B. After mixing evenly, add solution D dropwise and continue stirring at room temperature for 24 hours. After the reaction is completed, filter and wash with anhydrous ethanol and deionized water, and then dry at 60°C for 12 hours to obtain a transition metal phosphide Pt-based composite catalyst.
[0059] Example 2: Same as Example 1, except that the hexadecyltrimethylammonium bromide in step S2 is replaced by polyvinylpyrrolidone. Example 3: Same as Example 1, except that the hexadecyltrimethylammonium bromide in step S2 is replaced by sodium dodecylbenzenesulfonate.
[0060] The transition metal phosphide Pt-based composite catalysts prepared in Example 1, Example 2 and Example 3 were subjected to XRD detection and electron microscope scanning. The results are as follows: Figure 1-Figure 4 As shown, Figure 1 The XRD patterns of hydrangea-shaped Pt / Fe2P-CoP-NDC (h), spherical Pt / Fe2P-CoP-NDC (s) and lamellar Pt / Fe2P-CoP-NDC (f) composite catalysts are shown in Figure 1. Compared with the standard cards, it can be found that although some diffraction peaks overlap, the diffraction peaks of the three catalysts still correspond well to the standard peaks of each substance. Moreover, the XRD patterns of the flake, hydrangea and porous spherical composite catalysts have similar peak types, indicating that the three catalysts have the same material composition. Figure 2 , Figure 3 and Figure 4 These are SEM images of three catalysts with different morphologies. It can be seen from the figure that the three catalysts are respectively lamellar, hydrangea-shaped and spherical, proving that the morphology and structure of the catalysts are precisely controlled.
[0061] Figure 5 The CV curves of three catalysts with different morphologies are shown in Figure 2. According to the calculation, the ECSAs of the hydrangea-shaped Pt / Fe2P-CoP-NDC (h), spherical Pt / Fe2P-CoP-NDC (s) and lamellar Pt / Fe2P-CoP-NDC (f) composite catalysts are 75.8 m 2 ·g -1 、97.6m 2 ·g -1 and 51.4m 2 ·g -1 . Figure 6 The mass activity and specific activity of three catalysts with different morphologies are shown. The peak current density of spherical Pt / Fe2P-CoP-NDC(s) is 1292 mA·mg -1 Pt , respectively, lamellar Pt / Fe2P-CoP-NDC(f)(508mA·mg -1Pt )、hydrangea-shaped Pt / Fe2P-CoP-NDC(h)(917mA·mg -1 Pt ) is 2.54 and 1.41 times the current density of the composite catalyst. Figure 7 The specific activity curves of the three catalysts show that the specific activity of the spherical catalyst is 1.32 mA cm -2 , better than Pt / Fe2P-CoP-NDC(f)(0.99mA·cm -2 ) and Pt / Fe2P-CoP-NDC(h)(1.21mA·cm -2 ) catalyst. At the same time, Figure 8-Figure 11 The results of CA tests and 1000-cycle cyclic stability tests also confirmed that spherical catalysts have better catalytic stability than flake-shaped and hydrangea-shaped catalysts, indicating that the morphology and structure of the catalyst have a key influence on the catalytic performance of the catalyst. Regulating the morphology and structure of Pt-based catalysts is of great significance to the design and development of high-performance composite catalysts.
[0062] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which are all covered by the protection scope of the present invention.
Claims
1. A method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology, characterized in that: It includes the following steps: S1. Preparation of Fe-DCD precursor: Dissolve ferric nitrate and dicyandiamide in ethanol solution, heat in a water bath to 70-90°C, and continue stirring until ethanol is completely evaporated to obtain Fe-DCD precursor; S2. Preparation of Fe-Co-DCD precursor: The precursor Fe-DCD, surfactant and cobalt nitrate prepared in step S1 are dissolved in methanol to obtain solution A; the methanol solution of dimethylimidazole is slowly added to solution A and mixed evenly, and then transferred to a reactor and reacted at 110-130° C. for 10-14 hours to generate a Fe-Co-DCD precursor; S3. Preparation of composite support: After the Fe-Co-DCD precursor and triphenylphosphine were mixed and ground evenly, they were calcined at 580-620 ° C for 1.5-2.5 h in a nitrogen atmosphere, and then calcined at 780-820 ° C for 1.5-2.5 h to obtain a Fe2P-CoP-NDC composite support; S4. Preparation of composite catalyst: The Fe2P-CoP-NDC composite carrier obtained in step S3 is acid-etched, and Pt nanoparticles are loaded after acid etching to obtain a Pt / Fe2P-CoP-NDC composite catalyst.
2. The method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology according to claim 1, characterized in that: In step S1, the weight ratio of ferric nitrate to dicyandiamide is 1:3-5, and the volume ratio of the total mass of ferric nitrate and dicyandiamide to the ethanol solution is 1g:20-30ml.
3. The method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology according to claim 1, characterized in that: The surfactant in step S2 is any one of cetyltrimethylammonium bromide, polyvinylpyrrolidone or sodium dodecylbenzenesulfonate. If the surfactants are cetyltrimethylammonium bromide, polyvinylpyrrolidone and sodium dodecylbenzenesulfonate respectively, the morphologies of the prepared Pt / Fe2P-CoP-NDC composite catalyst are hydrangea-shaped, spherical and lamellar.
4. The method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology according to claim 1, characterized in that: In step S2, the weight ratio of the precursor Fe-DCD, the surfactant and the cobalt nitrate is 1:1.5-3:1.2-1.8, the mass volume ratio of dimethylimidazole to the methanol solution in the dimethylimidazole methanol solution is 0.2-0.4g:10ml; the volume ratio of the solution A to the dimethylimidazole methanol solution is 1.5-3:
1.
5. The method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology according to claim 1, characterized in that: The weight ratio of triphenylphosphine to Fe-DCD in step S3 is 3 to 5:
1.
6. The method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology according to claim 1, characterized in that: The heating rate in step S3 is 1.5-2.5°C / min.
7. The method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology according to claim 1, characterized in that: The specific operation of the acid etching in step S4 is: the Fe2P-CoP-NDC composite carrier is immersed in a 0.3-0.8MH2SO4 solution for acid etching for 50-70 minutes.
8. The method for synthesizing a transition metal phosphide Pt-based composite catalyst with adjustable morphology according to claim 1, characterized in that: The specific operation steps of loading Pt nanoparticles in step S4 are: S41. The Fe2P-CoP-NDC composite carrier is dispersed in deionized water and uniformly dispersed by ultrasonication, referred to as solution B, wherein the concentration of the Fe2P-CoP-NDC composite carrier in solution B is 0.8 to 1.2 mg / ml; Dissolve trisodium citrate and 48.803 mM H2PtCl6-EG in deionized water, referred to as solution C, wherein the concentration of trisodium citrate in solution C is 4-6 mg / ml, and the volume ratio of H2PtCl6-EG to deionized water is 1:8-12; dissolve NaBH4 in deionized water, referred to as solution D, wherein the concentration of NaBH4 in solution D is 0.3-0.7 mg / ml; S42. While stirring at a speed of 400 to 700 r / min, slowly add solution C to solution B. After mixing evenly, add solution D dropwise. The volume ratio of solution B, solution C and solution D is 3 to 5:1:1.2 to 2. Continue stirring at room temperature for 22 to 26 hours. After the reaction is completed, filter and wash with anhydrous ethanol and deionized water. Then, dry at a temperature of 55 to 65°C for 10 to 14 hours to obtain a transition metal phosphide Pt-based composite catalyst.
Citation Information
Patent Citations
Preparation method of layered cobalt-zinc double hydroxide-graphene compound supercapacitor electrode
CN106206055A
Preparation method and application of aluminum-iron co-doped cobalt phosphide nanoparticle / graphene composite material
CN110589785A
Method for preparing carbon carrier loaded platinum-based nanoparticle catalyst under assistance of functional small molecules
CN114904516A
Preparation method for iron-cobalt phosphide / carbon composite material having layered structure, and button cell
WO2023115503A1