Membrane electrode and preparation method and application thereof

By designing catalytic particles with larger particle sizes and first sublayers with low loads, catalytic particles with smaller particle sizes and second sublayers with high loads in the membrane electrode, the problem of poor durability of the membrane electrode is solved. , significantly improves the durability and performance of the membrane electrode.

CN119050388APending Publication Date: 2024-11-29DONGFENG MOTOR GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411044047.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The durability of the membrane electrode is poor, resulting in the dissolution and re-precipitation of catalytic particles near the proton exchange membrane, forming a depletion zone of catalytic body, resulting in slow proton transport and ohmic loss.

Method used

A membrane electrode is designed, including a proton exchange membrane and a catalytic layer. The catalytic layer consists of a first sub-layer and a second sub-layer. The first sub-layer adopts catalytic particles with larger particle sizes and low loading when close to the proton exchange membrane. The second sub-layer away from the proton exchange membrane uses catalytic particles with smaller particle size and high loading, and uses ultrasonic spray spray to form a film electrode.

Benefits of technology

The durability of the membrane electrode is significantly improved, the formation of catalytic body depletion zone is avoided, the catalytic body loss is reduced, the transport resistance of catalytic body ions near the proton exchange membrane is increased, and the service life of the membrane electrode is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050388A_ABST
    Figure CN119050388A_ABST
Patent Text Reader

Abstract

The invention relates to a membrane electrode and a preparation method and application thereof, and belongs to the technical field of fuel cells. The particle size of the catalytic particles close to one side of the proton exchange membrane is relatively large, and the catalytic particles close to the membrane are inhibited from being dissolved and re-precipitated, so that ohmic loss caused by slow proton transportation due to formation of a catalytic body depletion zone is avoided; meanwhile, the content of the ionic polymer close to one side of the proton exchange membrane is relatively low, so that the transport resistance of catalytic body ions close to the proton exchange membrane can be remarkably increased, the diffusion of the catalytic body ions to the proton exchange membrane is hindered, and the loss of the catalytic body is favorably reduced; meanwhile, the loading capacity of the catalytic body close to one side of the proton exchange membrane is reduced, the ion loading capacity of the catalytic body far away from one side of the proton exchange membrane is improved, diffusion of catalytic body ions to the proton exchange membrane is hindered, loss of the catalytic body is reduced, and therefore the durability of the membrane electrode is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of fuel cell technology, and in particular to a membrane electrode and a preparation method and application thereof. Background Art

[0002] Since proton exchange membrane fuel cells use hydrogen as fuel and do not generate pollutants such as SOx, NOx, CO, CO2, etc., they provide a new solution to the environmental and energy problems caused by automobiles.

[0003] The membrane electrode assembly is the core part of the proton exchange membrane fuel cell. It is the core component of the fuel cell to generate current. It is known as the "heart" of the fuel cell and is the core place where electrochemical reactions occur. The quality of the membrane electrode determines the performance of the battery. The membrane electrode assembly is usually composed of a proton exchange membrane, an anode catalyst layer, a cathode catalyst layer, an anode gas diffusion layer, and a cathode gas diffusion layer. At present, the durability of fuel cells still has a lot of room for improvement. Summary of the invention

[0004] The present application provides a membrane electrode and a preparation method and application thereof to improve the current problem of poor durability of membrane electrodes.

[0005] In the first aspect, the present application provides a membrane electrode, which includes a proton exchange membrane and a catalyst layer, the catalyst layer includes a first sublayer and a second sublayer, the first sublayer is arranged between the proton exchange membrane and the second sublayer; the first sublayer includes first catalytic particles and a first ionic polymer, the first catalytic particles include a first carrier and a first catalytic body loaded on the first carrier; the second sublayer includes second catalytic particles and a second ionic polymer, the second catalytic particles include a second carrier and a second catalytic body loaded on the second carrier; the particle size of the first catalytic particles is larger than the particle size of the second catalytic particles, the loading of the first catalytic body in the first sublayer is smaller than the loading of the second catalytic body in the second sublayer, and the content of the first ionic polymer in the first sublayer is smaller than the content of the second ionic polymer in the second sublayer.

[0006] As an optional embodiment, the particle size of the first catalytic particles is greater than 4 nm; and / or

[0007] The particle size of the second catalytic particles is 2 nm to 3 nm.

[0008] As an optional embodiment, the loading amount of the first catalytic body in the first sub-layer is 0.05 mg / cm 2 ~0.15mg / cm 2 ; and / or

[0009] The loading of the second catalytic body in the second sub-layer is 0.25 mg / cm 2 ~0.35mg / cm 2 .

[0010] As an optional embodiment, the weight ratio of the first ionic polymer in the first sublayer to the first carrier is 0.6 to 0.8; and / or

[0011] The weight ratio of the second ionic polymer to the second carrier in the second sublayer is 0.8 to 1.2.

[0012] As an optional embodiment, the mass content of the first catalytic body in the first catalytic particles is 30% to 70%; and / or

[0013] The first carrier comprises a carbon material; and / or

[0014] The first catalytic body includes platinum or a platinum-based material.

[0015] As an optional embodiment, the mass content of the second catalytic body in the second catalytic particles is 30% to 70%; and / or

[0016] The second carrier comprises a carbon material; and / or

[0017] The second catalytic body includes platinum or a platinum-based material.

[0018] In a second aspect, the present application provides a method for preparing the membrane electrode provided in the first aspect, the method comprising:

[0019] mixing first catalyst particles, a first ionic polymer, and a dispersant to obtain a first slurry;

[0020] mixing second catalyst particles, a second ionic polymer, and a dispersant to obtain a second slurry;

[0021] The first slurry and the second slurry are sequentially applied to a proton exchange membrane to form a first sublayer and a second sublayer to obtain a membrane electrode.

[0022] As an optional embodiment, the dispersant includes at least one of ethanol, n-propanol, isopropanol, ethyl acetate, n-butanol and hexafluoroisopropanol; and / or

[0023] The first ionic polymer and the second ionic polymer are Nafion solutions; and / or

[0024] The mass concentration of the Nafion solution is 4% to 25%.

[0025] As an optional implementation, the coating method includes ultrasonic spray coating.

[0026] In a third aspect, the present application provides a fuel cell, comprising the membrane electrode provided in the first aspect.

[0027] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0028] The membrane electrode provided in the embodiment of the present application adopts catalytic particles with larger particle size (such as Pt / C particles) in the first sublayer close to the proton exchange membrane, and the catalytic body (such as Pt) loading and ion polymer content are both low, and catalytic particles with smaller particle size are adopted in the second sublayer far from the proton exchange membrane, and the catalytic body loading and ion polymer content are both high. The catalytic particles on the side close to the proton exchange membrane have larger particle size, which inhibits the formation of a catalytic body depletion zone and causes ohmic loss due to the dissolution and reprecipitation of catalytic particles near the membrane, thereby avoiding the formation of a catalytic body depletion zone and causing slow proton transport; the ion polymer content on the side close to the proton exchange membrane is low, which can significantly increase the catalytic body ions (such as Pt) near the proton exchange membrane. 2+ )'s transport resistance hinders the diffusion of catalyst ions to the proton exchange membrane, which helps to reduce the loss of catalyst body; reducing the catalyst body loading on the side close to the proton exchange membrane and increasing the catalyst body ion loading on the side away from the proton exchange membrane is beneficial to hinder the diffusion of catalyst body ions to the proton exchange membrane, which helps to reduce the loss of catalyst body, thereby significantly improving the durability of the membrane electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0031] Figure 1 A flowchart of the method provided in the embodiment of the present application. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0034] An embodiment of the present application provides a membrane electrode, which includes a proton exchange membrane and a catalyst layer, the catalyst layer includes a first sublayer and a second sublayer, the first sublayer is arranged between the proton exchange membrane and the second sublayer; the first sublayer includes first catalytic particles and a first ionic polymer, the first catalytic particles include a first carrier and a first catalytic body loaded on the first carrier; the second sublayer includes second catalytic particles and a second ionic polymer, the second catalytic particles include a second carrier and a second catalytic body loaded on the second carrier; the particle size of the first catalytic particles is larger than the particle size of the second catalytic particles, the loading of the first catalytic body in the first sublayer is smaller than the loading of the second catalytic body in the second sublayer, and the content of the first ionic polymer in the first sublayer is smaller than the content of the second ionic polymer in the second sublayer.

[0035] The membrane electrode adopts catalytic particles with larger particle size (such as Pt / C particles) in the first sublayer close to the proton exchange membrane, and the catalytic body (such as Pt) loading and ion polymer content are both low, and catalytic particles with smaller particle size are adopted in the second sublayer far from the proton exchange membrane, and the catalytic body loading and ion polymer content are both high. The catalytic particles on the side close to the proton exchange membrane are larger in particle size, which inhibits the formation of a catalytic body depletion zone and causes ohmic loss due to the dissolution and reprecipitation of catalytic particles near the membrane, thereby avoiding the formation of a catalytic body depletion zone and causing slow proton transport; the ion polymer content on the side close to the proton exchange membrane is lower, which can significantly increase the catalytic body ions (such as Pt 2+ )'s transport resistance hinders the diffusion of catalyst ions to the proton exchange membrane, which helps to reduce the loss of catalyst body; reducing the catalyst body loading on the side close to the proton exchange membrane and increasing the catalyst body ion loading on the side away from the proton exchange membrane is beneficial to hinder the diffusion of catalyst body ions to the proton exchange membrane, which helps to reduce the loss of catalyst body, thereby significantly improving the durability of the membrane electrode.

[0036] In some embodiments, the particle size of the first catalytic particle is greater than 4nm; the particle size of the second catalytic particle is 2nm to 3nm. By controlling the particle size of the first catalytic particle to be greater than 4nm and the particle size of the second catalytic particle to be 2nm to 3nm, it is possible to better suppress the dissolution and reprecipitation of the catalytic particles near the membrane, thereby avoiding the formation of a catalytic body depletion zone, which leads to slow proton transport and ohmic loss.

[0037] For example, the particle size of the first catalytic particle can be 4 nm, 4.5 nm, 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm, 8 nm, 8.5 nm, 9 nm, 9.5 nm or 10 nm, etc., and it can also be any value within the range of greater than 4 nm. The particle size of the second catalytic particle can be 2 nm, 2.1 nm, 2.2 nm, 2.3 nm, 2.4 nm, 2.5 nm, 2.6 nm, 2.7 nm, 2.8 nm, 2.9 nm or 3 nm, etc., and it can also be any value within the range of 2 nm to 3 nm.

[0038] In some embodiments, the loading of the first catalytic body in the first sublayer is 0.05 mg / cm 2 ~0.15mg / cm 2 The loading of the second catalytic body in the second sublayer is 0.25 mg / cm 2 ~0.35mg / cm 2 By controlling the loading of the first catalyst body to 0.05 mg / cm 2 ~0.15mg / cm 2 The loading of the second catalyst body is 0.25 mg / cm 2 ~0.35mg / cm 2 , which is beneficial to hinder the diffusion of catalyst body ions to the proton exchange membrane and helps to reduce the loss of catalyst body.

[0039] For example, the loading amount of the first catalytic body in the first sub-layer may be 0.05 mg / cm 2 , 0.07mg / cm 2 , 0.09mg / cm 2 , 0.11mg / cm 2 , 0.13mg / cm 2 or 0.15mg / cm 2 etc., which can also be 0.05 mg / cm 2 ~0.15mg / cm 2 The loading of the second catalytic body in the second sub-layer can be 0.25 mg / cm 2 , 0.27mg / cm 2 , 0.29mg / cm2 , 0.31mg / cm 2 , 0.33mg / cm 2 or 0.35mg / cm 2 etc., which can also be 0.25 mg / cm 2 ~0.35mg / cm 2 Any value in the range.

[0040] In some embodiments, the weight ratio of the first ion polymer in the first sublayer to the first carrier is 0.6 to 0.8; the weight ratio of the second ion polymer in the second sublayer to the second carrier is 0.8 to 1.2. By controlling the weight ratio of the first ion polymer to the first carrier to be 0.6 to 0.8 and the weight ratio of the second ion polymer to the second carrier to be 0.8 to 1.2, the transport resistance of the catalyst body ions near the proton exchange membrane can be significantly increased, the diffusion of the catalyst body ions to the proton exchange membrane is hindered, and it is helpful to reduce the catalyst body loss.

[0041] Exemplarily, the weight ratio of the first ionic polymer to the first carrier in the first sublayer can be 0.6, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79 or 0.8, etc., and it can also be any value in the range of 0.6 to 0.8. The weight ratio of the second ionic polymer to the second carrier in the second sublayer can be 0.8, 0.85, 0.9, 0.95, 1.00, 1.05, 1.10, 1.15 or 1.2, etc., and it can also be any value in the range of 0.8 to 1.2.

[0042] In some embodiments, the mass content of the first catalytic body in the first catalytic particle is 30% to 70%; the first carrier includes a carbon material; and the first catalytic body includes platinum or a platinum-based material.

[0043] Exemplarily, the mass content of the first catalytic body in the first catalytic particle can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65% or 70%, etc., and it can also be any value within the range of 30% to 70%.

[0044] In some embodiments, the mass content of the second catalytic body in the second catalytic particle is 30% to 70%; the second carrier includes a carbon material; and the second catalytic body includes platinum or a platinum-based material.

[0045] Exemplarily, the mass content of the second catalytic body in the second catalytic particle can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65% or 70%, etc., and it can also be any value within the range of 30% to 70%.

[0046] Figure 1 A flow chart of the method provided in the embodiment of the present application is as follows: Figure 1 As shown, based on a general inventive concept, an embodiment of the present application also provides a method for preparing the membrane electrode provided in the first aspect.

[0047] The method is used for preparing the above-mentioned membrane electrode. The specific content of the membrane electrode can refer to the above-mentioned embodiment. Since the method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.

[0048] In some embodiments, the method comprises:

[0049] S1. mixing the first catalyst particles, the first ionic polymer and the dispersant to obtain a first slurry;

[0050] In some embodiments, the dispersant includes at least one of ethanol, n-propanol, isopropanol, ethyl acetate, n-butanol and hexafluoroisopropanol; the first ion polymer is a Nafion solution, and the mass concentration of the Nafion solution is 4% to 25%.

[0051] Specifically, in this embodiment, the wetted first catalyst particles Pt / C catalyst are stirred and mixed with a dispersant, and then an ionic polymer solution is added to the resulting mixed solution to obtain a first slurry, wherein the Pt / C catalyst includes a Pt / C catalyst with a platinum content of 30%-70%, and the particle size of the Pt particles in the catalyst is greater than 4nm.

[0052] S2. mixing the second catalyst particles, the second ionic polymer and the dispersant to obtain a second slurry;

[0053] In some embodiments, the dispersant includes at least one of ethanol, n-propanol, isopropanol, ethyl acetate, n-butanol and hexafluoroisopropanol; the second ionic polymer is a Nafion solution, and the mass concentration of the Nafion solution is 4% to 25%.

[0054] Specifically, in this embodiment, the wetted second catalyst particles Pt / C catalyst are stirred and mixed with a dispersant, and then an ionic polymer solution is added to the resulting mixed solution to obtain a second slurry, wherein the Pt / C catalyst includes a Pt / C catalyst with a platinum content of 30%-70%, and the particle size of the Pt particles in the catalyst is 2 to 3 nm.

[0055] S3. Sequentially apply the first slurry and the second slurry to a proton exchange membrane to form a first sublayer and a second sublayer to obtain a membrane electrode.

[0056] In some embodiments, the coating method includes ultrasonic spraying.

[0057] Specifically, in this embodiment, the first slurry is loaded into a spray coating barrel, the barrel is turned on for stirring, and the first slurry in the barrel is sprayed on the proton exchange membrane to preliminarily obtain the first sublayer, and the second slurry is loaded into a spray coating barrel, the barrel is turned on for stirring; the second slurry in the barrel is sprayed on the first sublayer to obtain the second sublayer. In the first sublayer, the platinum loading is 0.05-0.15 mg / cm 2 , the weight ratio of ionic polymer to carbon carrier (I / C) is 0.6-0.8. In the second sublayer, the platinum loading is 0.25-0.35 mg / cm2, and the weight ratio of ionic polymer to carbon carrier (I / C) is 0.8-1.2. The stirring speed of the spray barrel is 110-150 rpm. Too low stirring speed will increase the risk of sedimentation, and too high stirring speed will cause bubbles in the slurry.

[0058] In some embodiments, the mixing and dispersing method includes one or more combinations of mechanical stirring, water bath ultrasound and probe ultrasound after mixing, the mixing and dispersing time is 0.5 to 3 hours, and the dispersion process is always maintained in an ice water bath.

[0059] Based on a general inventive concept, an embodiment of the present application further provides a fuel cell, which includes the membrane electrode provided in the first aspect.

[0060] The fuel cell is realized based on the above-mentioned membrane electrode. The specific content of the membrane electrode can refer to the above-mentioned embodiments. Since the fuel cell adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0061] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0062] Example 1

[0063] A membrane electrode, the preparation process of which is as follows:

[0064] 1) Weigh 0.5 g of TKK 50.5% Pt / C (Pt particle size 4.7 nm) and add a small amount of water to wet the catalyst.

[0065] 2) Add 18.05 g of isopropanol to the mixed solution obtained in step 1, and stir mechanically under ice-water bath for half an hour to obtain a mixed solution.

[0066] 3) 3.807 g of the ionic polymer solution (I / C: 0.8) was added to the solution obtained in step 2 to obtain a first slurry.

[0067] 4) Add the first slurry prepared in step 3 into the spray coating barrel, start the barrel stirring, the stirring power is 10% of the maximum stirring power, take a 100×100 mm proton exchange membrane, and use the first slurry in the barrel to spray on a heating table at 90° C. to obtain a first sublayer (loading 0.15 mg / cm 2 ).

[0068] 5) Weigh 0.5 g of TKK 47% Pt / C (Pt particle size: 2.4 nm), and add a small amount of water to wet the catalyst.

[0069] 6) Add 19.79 g of isopropanol to the mixed solution obtained in step 5, and stir mechanically under ice-water bath for half an hour to obtain a mixed solution.

[0070] 7) 5.096 g of the ionic polymer solution (I / C: 1.0) was added to the solution obtained in step 6 to obtain a second slurry.

[0071] 8) Add the second slurry prepared in step 7 to the spray coating barrel, start the barrel stirring, the stirring power is 10% of the maximum stirring power, take a 100×100 mm proton exchange membrane, and use the second slurry in the barrel to spray on a heating table at 90° C. to obtain a second sublayer (loading 0.25 mg / cm 2 ).

[0072] Example 2

[0073] A membrane electrode, the preparation process of which is as follows:

[0074] 1) Weigh 0.5 g of TKK 50.5% Pt / C (Pt particle size 4.7 nm) and add a small amount of water to wet the catalyst.

[0075] 2) Add 16.77 g of isopropanol to the mixed solution obtained in step 1, and stir mechanically under ice-water bath for half an hour to obtain a mixed solution.

[0076] 3) 2.86 g of the ionic polymer solution (I / C: 0.6) was added to the solution obtained in step 2 to obtain a first slurry.

[0077] 4) Add the first slurry prepared in step 3 into the spray coating barrel, start the barrel stirring, the stirring power is 10% of the maximum stirring power, take a 100×100 mm proton exchange membrane, and use the first slurry in the barrel to spray on a heating table at 90° C. to obtain a first sublayer (loading 0.1 mg / cm 2 ).

[0078] 5) Weigh 0.5 g of TKK 47% Pt / C (Pt particle size: 2.4 nm), and add a small amount of water to wet the catalyst.

[0079] 6) Add 21.16 g of isopropanol to the mixed solution obtained in step 5, and stir mechanically under ice-water bath for half an hour to obtain a mixed solution.

[0080] 7) 6.115 g of the ionic polymer solution (I / C: 1.2) was added to the solution obtained in step 6 to obtain a second slurry.

[0081] 8) Add the second slurry prepared in step 7 to the spray coating barrel, start the barrel stirring, the stirring power is 10% of the maximum stirring power, take a 100×100 mm proton exchange membrane, and use the second slurry in the barrel to spray on a heating table at 90° C. to obtain a second sublayer (loading 0.3 mg / cm 2 ).

[0082] Comparative Example 1

[0083] A membrane electrode, the preparation process of which is as follows:

[0084] 1) Weigh 0.5 g of TKK 47% Pt / C (Pt particle size 2.4 nm) and add a small amount of water to wet the catalyst.

[0085] 2) Add 21.34 g of isopropanol to the mixed solution obtained in step 1, and stir mechanically under ice-water bath for half an hour to obtain a mixed solution.

[0086] 3) Add 8.215 g of B ion polymer solution (ionomer content 5.2%) to the solution obtained in step 2 to obtain a catalyst layer slurry.

[0087] 4) Add the slurry prepared in step 3 into the spray barrel, start the barrel stirring, the stirring power is 10% of the maximum stirring power, take a 100×100 mm proton exchange membrane, and use the spraying method on a heating table at 90°C to spray the slurry in the barrel to obtain a catalyst layer (loading 0.4 mg / cm 2 ).

[0088] Comparative Example 2

[0089] A membrane electrode, the preparation process of which is as follows:

[0090] 1) Weigh 0.5 g of TKK 50.5% Pt / C (Pt particle size 4.7 nm) and add a small amount of water to wet the catalyst.

[0091] 2) Add 16.77 g of isopropanol to the mixed solution obtained in step 1, and stir mechanically under ice-water bath for half an hour to obtain a mixed solution.

[0092] 3) Add 8.215 g of B ion polymer solution (ionomer content 5.2%) to the solution obtained in step 2 to obtain a catalyst layer slurry.

[0093] 4) Add the slurry prepared in step 3 into the spray barrel, start the barrel stirring, the stirring power is 10% of the maximum stirring power, take a 100×100 mm proton exchange membrane, and use the spraying method on a heating table at 90°C to spray the slurry in the barrel to obtain a catalyst layer (loading 0.4 mg / cm 2 ).

[0094] Comparative Example 3

[0095] This comparative example is the same as Example 2 except that the first sublayer and the second sublayer are swapped.

[0096] The membrane electrodes provided in the embodiments and comparative examples were used to perform durability tests. The electrochemical active area and performance decay rate after the durability test (30,000 cycles of 0.6-0.95) are shown in the following table.

[0097]

[0098]

[0099] It can be seen from the above table that the membrane electrode prepared by the method provided in the embodiment of the present application has good durability.

[0100] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0101] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b and c can be single or multiple.

[0102] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A membrane electrode, characterized in that: The membrane electrode comprises a proton exchange membrane and a catalyst layer, the catalyst layer comprises a first sublayer and a second sublayer, the first sublayer is arranged between the proton exchange membrane and the second sublayer; the first sublayer comprises first catalytic particles and a first ionic polymer, the first catalytic particles comprise a first carrier and a first catalytic body loaded on the first carrier; the second sublayer comprises second catalytic particles and a second ionic polymer, the second catalytic particles comprise a second carrier and a second catalytic body loaded on the second carrier; the particle size of the first catalytic particles is larger than the particle size of the second catalytic particles, the loading amount of the first catalytic body in the first sublayer is smaller than the loading amount of the second catalytic body in the second sublayer, and the content of the first ionic polymer in the first sublayer is smaller than the content of the second ionic polymer in the second sublayer.

2. The membrane electrode according to claim 1, characterized in that: The particle size of the first catalytic particles is greater than 4 nm; and / or The particle size of the second catalytic particles is 2 nm to 3 nm.

3. The membrane electrode according to claim 1, characterized in that: The loading of the first catalytic body in the first sublayer is 0.05 mg / cm 2 ~0.15mg / cm 2 ; and / or The loading of the second catalytic body in the second sub-layer is 0.25 mg / cm 2 ~0.35mg / cm 2 .

4. The membrane electrode according to claim 1, characterized in that: The weight ratio of the first ionic polymer in the first sublayer to the first carrier is 0.6 to 0.8; and / or The weight ratio of the second ionic polymer to the second carrier in the second sublayer is 0.8 to 1.

2.

5. The membrane electrode according to claim 1, characterized in that: The mass content of the first catalytic body in the first catalytic particle is 30% to 70%; and / or The first carrier comprises a carbon material; and / or The first catalytic body includes platinum or a platinum-based material.

6. The membrane electrode according to claim 1, characterized in that: The mass content of the second catalytic body in the second catalytic particles is 30% to 70%; and / or The second carrier comprises a carbon material; and / or The second catalytic body includes platinum or a platinum-based material.

7. A method for preparing a membrane electrode according to any one of claims 1 to 6, characterized in that: The method comprises: mixing first catalyst particles, a first ionic polymer, and a dispersant to obtain a first slurry; mixing second catalyst particles, a second ionic polymer, and a dispersant to obtain a second slurry; The first slurry and the second slurry are sequentially applied to a proton exchange membrane to form a first sublayer and a second sublayer to obtain a membrane electrode.

8. The method for preparing a membrane electrode according to claim 7, characterized in that: The dispersant comprises at least one of ethanol, n-propanol, isopropanol, ethyl acetate, n-butanol and hexafluoroisopropanol; and / or The first ionic polymer and the second ionic polymer are Nafion solutions; and / or The mass concentration of the Nafion solution is 4% to 25%.

9. The method for preparing a membrane electrode according to claim 7, characterized in that: The coating method includes ultrasonic spray coating.

10. A fuel cell, characterized in that: The fuel cell comprises the membrane electrode according to any one of claims 1 to 6.