Lithium-supplementing positive electrode material as well as preparation method and application thereof
By in-situ composite of carbon oxygen lithiide lithium replenishment particles in the positive electrode material of lithium-ion battery and adopting carbon cladding, the problem of gas production and side reaction risks of the battery after lithium replenishment is solved, and the cycle life and safety performance of the battery are improved.
Patent Information
- Application Number
- CN202411340742.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-29
AI Technical Summary
After lithium replenishment, existing lithium-ion batteries have poor contact with the positive electrode active substance particles, resulting in high decomposition voltage and gas production problems. The contact between the residues of the high-oxidation lithium replenishment and the electrolyte increases the risk of side reactions, especially It is even more serious in high temperature environments.
By in-situ composite of carbon oxygen lithiide lithium replenishing particles to the core of the positive electrode active material and adopting a carbon cladding layer, the size of lithium replenishing particles is reduced, contact and conductivity are improved, decomposition voltage and water absorption failure rate are reduced, and gel phenomenon is avoided and side reactions.
It effectively reduces the gas production problems of the battery during use, improves the electron conduction and ion conduction capabilities, extends the cycle life and safety performance of the battery, and reduces the preparation cost.
Smart Images

Figure CN119050509A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of lithium-ion batteries, and in particular to a lithium-supplemented cathode material, a preparation method thereof, and an application thereof. Background Art
[0002] The lithium supplementation technology is an effective means to improve the energy density of lithium-ion batteries, while improving the battery cycle life and energy storage performance. The commonly used existing lithium supplementation technologies include negative electrode lithium supplementation, positive electrode lithium supplementation, electrolyte lithium supplementation, separator lithium supplementation, current collector lithium supplementation, and electrochemical lithium supplementation. Among them, positive electrode lithium supplementation is one of the most commonly used means. Currently, the method for positive electrode lithium supplementation is usually to directly add a lithium supplement agent to the positive electrode slurry during the homogenization process. This will result in poor contact between the lithium supplement agent and the positive electrode active material particles, resulting in a higher decomposition voltage, and further causing problems such as gas generation in the battery after lithium supplementation; moreover, the lithium supplement residue in the high oxidation state remaining inside the positive electrode sheet contacting the electrolyte will increase the risk of side reactions, and further increase the risk of gas generation in the battery during use, especially in a high-temperature environment. Summary of the Invention
[0003] In view of this, the present application provides a lithium-supplemented cathode material, a preparation method thereof, and an application thereof. By in-situ compounding lithium carbon oxide particles on the core of the positive electrode active material, the size of the lithium supplement particles in the lithium-supplemented cathode material is much smaller than that of the lithium supplement agent conventionally added to the positive electrode active slurry, thereby effectively reducing the risk of gelation of the positive electrode active slurry caused by residual alkali on the surface of the lithium supplement agent, and effectively improving the electron conduction ability and ion conduction ability of the lithium-supplemented cathode material. Moreover, the carbon-containing coating layer can effectively slow down the rate of water absorption failure of the lithium supplement particles. In addition, the structure of the lithium-supplemented cathode material can also effectively reduce the decomposition voltage, thereby solving the problem of gas generation in the later use process of the battery.
[0004] The first aspect of the present application provides a lithium-supplemented cathode material, which includes an active material core and a coating layer coated on the surface of the active material core. The coating layer includes lithium supplement particles and carbon; the active material core includes Li x1 Fe y1 PO4, LiFe x2 Mn 1-x2 PO4, LiNi x3 Co y3 Mn 1-x3-y3 O2 and LiNi x4 Co y4 Al 1-x4-y4 O2, one or more of them, where 0.9 ≤ x1 ≤ 1.1, 0.9 ≤ y1 ≤ 1.1, 0 < x2 < 1, 0 < x3 < 1, 0 < y3 < 1, 0 < x4 < 1, 0 < y4 < 1; the lithium supplement particles include Lia C b O c , where 0<a≤6, 0<b≤6, 0<c≤6.
[0005] In the embodiment of the present application, the carbon is coated on the surface of the active material core and / or the lithium supplement particle.
[0006] In an embodiment of the present application, at least part of the lithium supplement particles are in-situ grown on the surface of the active material core.
[0007] In an embodiment of the present application, the lithium supplement particles include one or more of Li2C4O4, Li2CO3, Li2C2O4 and Li6C6O6.
[0008] In an embodiment of the present application, the mass ratio of the lithium supplement particles to the active material core is (0.1-10):100.
[0009] In the implementation manner of the present application, the mass percentage of the carbon in the lithium-supplementing positive electrode material is 0.1%-5%.
[0010] In the embodiment of the present application, the particle size of the active material core is 0.02 μm-50 μm; the particle size of the lithium supplement particle is 0.01 μm-10 μm.
[0011] In the embodiment of the present application, when the active material core is Li x1 Fe y1 PO4 and / or LiFe x2 Mn 1-x2 PO4, the particle size of the active material core is 0.02 μm-15 μm, and the particle size of the lithium supplement particles is 0.01 μm-8 μm; when the active material core is LiNi x3 Co y3 Mn 1-x3-y3 O2 and / or LiNi x4 Co y4 Al 1-x4-y4 When O2 is used, the particle size of the active material core is 0.4 μm-50 μm, and the particle size of the lithium supplement particle is 0.01 μm-10 μm.
[0012] In the embodiment of the present application, the specific surface area of the lithium-supplementing positive electrode material is 0.2 m 2 / g-20m 2 / g.
[0013] The second aspect of the present application provides a method for preparing the lithium-supplemented positive electrode material provided in the first aspect of the present application, comprising the following steps:
[0014] Mixing a lithium source, a phosphorus source, an iron source and a carbon source to obtain a lithium-supplementing positive electrode material precursor; or, mixing a lithium source, a phosphorus source, an iron source, a manganese source and a carbon source to obtain a lithium-supplementing positive electrode material precursor;
[0015] Sintering the lithium-supplementing positive electrode material precursor to obtain a lithium-supplementing positive electrode material;
[0016] Or, include:
[0017] Mixing a lithium source, a nickel source, a cobalt source, and a manganese source or an aluminum source to obtain a lithium-supplemented positive electrode material precursor;
[0018] The lithium-replenishing positive electrode material precursor is sintered, and then mixed with a carbon source and subjected to secondary sintering to obtain the lithium-replenishing positive electrode material.
[0019] In the embodiment of the present application, the temperature of the sintering treatment is 600°C-900°C, and the sintering time is 6h-24h; the temperature of the secondary sintering treatment is 700°C-1000°C, and the sintering time is 2h-8h.
[0020] The third aspect of the present application provides a positive electrode sheet, which includes a current collector and a positive electrode active layer loaded on the current collector, and the positive electrode active layer includes the lithium-supplementing positive electrode material provided in the first aspect of the present application or the lithium-supplementing positive electrode material prepared by the preparation method provided in the second aspect of the present application.
[0021] A fourth aspect of the present application provides a lithium-ion battery, which includes the positive electrode sheet provided in the third aspect of the present application.
[0022] A fifth aspect of the present application provides an electrical device, which includes a lithium-ion battery as provided in the fourth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of the cross-sectional structure of a lithium-supplementing positive electrode material provided in one embodiment of the present application;
[0024] Figure 2 This is a schematic diagram of the cross-sectional structure of a lithium-supplementing positive electrode material provided in yet another embodiment of the present application.
[0025] Description of Figure Numbers
[0026] 100-lithium-supplemented positive electrode material; 101-active material core; 102-lithium-supplemented particles; 103-carbon. DETAILED DESCRIPTION
[0027] The present application is further described in detail below in conjunction with preferred embodiments, but the protection scope of the present application is not limited to the following specific embodiments.
[0028] In the present application, all professional terms have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present application.
[0029] Lithium replenishment technology is an effective means to improve the energy density of lithium-ion batteries and improve the battery cycle life and energy storage performance. The commonly used lithium replenishment technologies include negative electrode lithium replenishment, positive electrode lithium replenishment, electrolyte lithium replenishment, diaphragm lithium replenishment, current collector lithium replenishment and electrochemical lithium replenishment. Among them, positive electrode lithium replenishment is one of the most commonly used methods. At present, the method for positive electrode lithium replenishment is usually to directly add the lithium replenisher to the positive electrode slurry in the homogenization process, which will make the contact between the lithium replenisher and the positive electrode active material particles poor, resulting in a high decomposition voltage, which in turn causes the battery to produce gas after lithium replenishment. Problems; and the lithium replenisher residues in a high oxidation state remaining inside the positive electrode sheet contact with the electrolyte will increase the risk of side reactions, thereby increasing the risk of gas production during use of the battery, especially in high temperature environments. In addition, the commonly used lithium replenishers are usually larger in particle size, about an order of magnitude larger than the positive electrode active material, which causes the lithium replenisher to shrink particles after the lithium replenishment is decomposed, resulting in collapsed holes around the lithium replenisher particles, which in turn causes the electrical contact between the positive electrode active materials in the positive electrode sheet to deteriorate.
[0030] See also Figure 1 The present application provides a lithium-supplementing positive electrode material 100, which includes an active material core 101 and a coating layer coated on the surface of the active material core 101, wherein the coating layer includes lithium-supplementing particles 102 and carbon 103. In the embodiment of the present application, the active material core 101 includes Li x1 Fe y1 PO4、LiFe x2 Mn 1-x2 PO4、LiNi x3 Co y3 Mn 1-x3-y3 O2 and LiNi x4 Co y4 Al 1-x4-y4One or more of O2, where 0.9 ≤ x1 ≤ 1.1, 0.9 ≤ y1 ≤ 1.1, 0 < x2 < 1, 0 < x3 < 1, 0 < y3 < 1, 0 < x4 < 1, 0 < y4 < 1. In some embodiments, x1 can be, for example, 0.9, 0.95, 1, 1.05, 1.1; y1 can be, for example, 0.9, 0.95, 1, 1.05, 1.1; x2 can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9; x3 can be, for example, 0.9, 0.95, 1, 1.05, 1.1; x2 can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9; y3 can be, for example, 0.9, 0.95, 1, 1.05, 1.1; x2 can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9; x4 can be, for example, 0.9, 0.95, 1, 1.05, 1.1; x2 can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9; y4 can be, for example, 0.9, 0.95, 1, 1.05, 1.1; x2 can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9.
[0031] In an embodiment of the present application, the lithium supplement particles 102 include Li a C b O c, wherein 0<a≤6, 0<b≤6, 0<c≤6. In some specific embodiments, a can be, for example, 1, 2, 3, 4, 5, 6; b can be, for example, 1, 2, 3, 4, 5, 6; c can be, for example, 1, 2, 3, 4, 5, 6. The lithium-supplementing positive electrode material of the present application provides a lithium-supplementing function by in-situ compounding of carbon oxide lithium-supplementing particles with the core of the positive electrode active material, without affecting the energy density of the core of the active material 101. Compared with the commonly used lithium replenishment method of directly adding the lithium replenisher to the active slurry, the lithium replenishment particles 102 are compounded with the active material core 101 in an in-situ growth manner, which can effectively improve the contact between the lithium replenishment particles 102 and the active material core 101. On the one hand, it can effectively reduce the decomposition starting voltage required for decomposition polarization, improve the decomposition rate, and effectively avoid the gas production problem of the battery during the recycling process, thereby improving the service life and safety performance of the battery; on the other hand, it can effectively shorten the electron transmission path and the lithium ion transmission path, and improve the electron conductivity and ion conductivity of the lithium replenishment positive electrode material 100. Compared with other conventional lithium-rich metal oxide lithium replenishers, the carbon oxygen lithium compound lithium replenishment particles used in this application have no metal oxide residue, no oxygen release, and no metal element dissolution, and have higher safety performance. Compared with lithium-rich metal oxides, the carbon oxygen lithium compound has a lower cost, which can further reduce the preparation cost of lithium replenishment positive electrode materials. In addition, carbon oxide lithium compounds have a very high theoretical lithium replenishment gram capacity and stable chemical properties. They will not absorb water and become ineffective, and are easier to produce and store, thereby broadening the application scenarios of lithium replenishment positive electrode materials and reducing production costs. However, the decomposition voltage of carbon oxide lithium compounds themselves is high and their conductivity is very poor, making it difficult to use them alone as a lithium replenishment agent. This application uses a coating layer containing carbon 103 to at least partially wrap the lithium replenishment particles 102 and the active material core 101. On the one hand, the lithium replenishment particles 102 and the active material core 101 are tightly combined, effectively reducing the decomposition voltage. On the other hand, the overall conductivity of the lithium replenishment positive electrode material can also be significantly improved. In this application, the decomposition voltage and decomposition rate can be measured by cyclic voltammetry.
[0032] In the embodiment of the present application, at least part of the lithium supplement particles 102 are in-situ grown on the surface of the active material core 101 .
[0033] In some embodiments of the present application, the structure of the lithium-supplemented positive electrode material 100 is as follows Figure 1As shown, it includes an active material core 101, lithium supplement particles 102 bonded to the surface of the active material core 101, and a carbon coating layer 103 coated on the active material core 101 and / or the surface of the lithium supplement particles 102, wherein the lithium supplement particles 102 are in-situ grown on the surface of the active material core 101. In some embodiments of the present application, the lithium supplement particles 102 are in direct contact with the surface of the active material core 101. The lithium supplement particles in the lithium supplement positive electrode material of this structure are larger in size, thereby making the specific surface area of the lithium supplement positive electrode material smaller and the stability of the lithium supplement positive electrode material better.
[0034] In some other embodiments of the present application, the structure of the lithium-supplemented positive electrode material 100 is as follows: Figure 2 As shown, it includes an active material core 101 and a coating layer coated on the surface of the active material core 101, wherein the coating layer includes lithium supplement particles 102 and carbon 103, and the lithium supplement particles 102 are distributed inside the coating layer formed by the carbon 103. In some embodiments of the present application, the lithium supplement particles 102 are not in direct contact with the surface of the active material core 101, and the lithium supplement particles 102 are connected to the surface of the active material core 101 through the carbon 103.
[0035] In the embodiment of the present application, carbon 103 is coated on the surface of the active material core 101 and / or the lithium supplement particles 102. In the embodiment of the present application, the coating of the active material core 101 and the lithium supplement particles 102 by carbon 103 can be complete or incomplete. The lithium supplement positive electrode material 100 of the present application effectively reduces the contact area between the lithium supplement particles 102 and the air through the coating of carbon 103, thereby reducing the rate of water absorption failure of the lithium supplement particles 102 and effectively avoiding the residual alkali on the surface of the lithium supplement particles and the positive electrode active slurry to mix and form agglomeration, gelation, etc., thereby improving the utilization rate and service life of the lithium supplement particles, reducing the cost of preparation, and further improving the electrochemical performance of the battery product. The coating of carbon 103 can also optimize the conductive network structure of the positive electrode lithium supplement material, ensure the electronic path of the lithium supplement particles 102 and the active material core 101, and ensure the conductivity of the lithium supplement positive electrode material 100 while adding the lithium supplement particles 102. In addition, it can also improve the lithium ion deintercalation path of the lithium supplement particles 102 and the active material core 101, and improve the ionic conductivity of the lithium supplement positive electrode material 100, thereby effectively reducing the decomposition voltage and accelerating the decomposition speed, effectively improving the decomposition efficiency, and alleviating the gas production problem during the use of the battery. And through the coating of carbon 103, the active material core 101 and the lithium supplement particles 102 are more closely combined, which can also reduce their decomposition voltage.
[0036] In the embodiment of the present application, the lithium-replenishing particles 102 include one or more of Li2C4O4, Li2CO3, Li2C2O4 and Li6C6O6. In some embodiments of the present application, the lithium-replenishing particles may be, for example, Li2C4O4 and Li2CO3. The present application can further enhance its lithium-replenishing efficiency by selecting suitable carbon oxide lithium compounds as lithium-replenishing particles. Compared with lithium-rich metal oxides, carbon oxide lithium-replenishing particles do not have any residue after being fully decomposed during the first charge, which effectively avoids the risk of metal dissolution during subsequent recycling of the battery. In addition, after the decomposition of the carbon oxide lithium-replenishing particles, a fine void structure will be formed in the positive electrode sheet, which increases the porosity of the electrode sheet, thereby improving the liquid retention performance of the positive electrode sheet, and improving the battery rate performance and cycle life.
[0037] In the embodiment of the present application, the mass ratio of the lithium supplement particles 102 and the active material core 101 is (0.1-10): 100. In some specific embodiments, the mass ratio of the lithium supplement particles 102 and the active material core 101 can be, for example, 0.1: 100, 0.2: 100, 0.3: 100, 0.5: 100, 0.8: 100, 1: 100, 2: 100, 3: 100, 4: 100, 5: 100, 6: 100, 7: 100, 8: 100, 9: 100, 10: 100. The present application can make the lithium supplement positive electrode material have a higher specific capacity while improving the utilization rate of the lithium supplement particles by controlling the mass ratio of the lithium supplement particles and the active material core within a suitable range, effectively avoiding the waste of the lithium supplement particles while avoiding the side reactions caused by the excessive amount of lithium supplement particles, so that the lithium supplement positive electrode material has better comprehensive performance and meets the application requirements of different scenarios.
[0038] In the embodiment of the present application, the mass percentage of carbon 103 in the lithium-supplementing positive electrode material 100 is 0.1%-5%. In some specific embodiments, the mass percentage of carbon 103 in the lithium-supplementing positive electrode material 100 can be, for example, 0.1%, 0.2%, 0.3%, 0.5%, 0.6%, 0.8%, 1%, 2%, 3%, 4%, 5%. The present application can control the thickness of the coating layer by reasonably controlling the carbon content in the lithium-supplementing positive electrode material, and can also comprehensively adjust the coating method and degree of carbon 103 for the active material core 101 and the lithium-supplementing particles 102, thereby regulating the power performance, cycle performance and storage performance of the battery to meet the different needs of the battery.
[0039] In the embodiment of the present application, the particle size of the active material core 101 is 0.02μm-50μm; the particle size of the lithium supplement particle 102 is 0.01μm-10μm. In some specific embodiments, the particle size of the active material core 101 can be, for example, 0.02μm, 0.05μm, 0.1μm, 0.5μm, 1μm, 5μm, 10μm, 20μm, 30μm, 40μm, 50μm; the particle size of the lithium supplement particle 102 can be, for example, 0.01μm, 0.02μm, 0.05μm, 0.1μm, 0.5μm, 1μm, 2μm, 5μm, 8μm, 10μm.
[0040] In some embodiments of the present application, the active material core 101 is Li x1 Fe y1 PO4 and / or LiFe x2 Mn 1-x2 PO4, the particle size of the active material core 101 is 0.02μm-15μm, and the particle size of the lithium supplement particle 102 is 0.01μm-8μm. In some specific embodiments, the particle size of the active material core 101 can be, for example, 0.02μm, 0.04μm, 0.05μm, 0.06μm, 0.08μm, 0.1μm, 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.8μm, 1μm, 2μm, 3μm, 4μm, 5μm, 8μm, 10μm, 12μm, 15μm; the particle size of the lithium supplement particle 102 can be, for example, 0.01μm, 0.02μm, 0.04μm, 0.05μm, 0.08μm, 0.1μm, 0.2μm, 0.4μm, 0.5μm, 0.8μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 5μm, 6μm, 8μm. In some embodiments, the particle size of the active material core 101 can be 0.2μm-5μm, and the particle size of the lithium supplement particle 102 is 0.02μm-3μm. When the active material is a lithium iron phosphate type or lithium iron manganese phosphate type positive electrode material, controlling the particle size of the active material core and the lithium supplement particle within the above range is not only beneficial to the processing of the lithium supplement positive electrode material particles, but also beneficial to improving the processing stability of the slurry during the preparation of the slurry, thereby further improving the specific capacity and rate performance of the lithium supplement positive electrode material and further reducing the decomposition voltage. In this application, the particle size specifically refers to the median particle size D50, that is, DV50, which refers to the particle size corresponding to when the cumulative particle size distribution percentage of the measured sample reaches 50%. The physical meaning is that particles with a particle size larger than it account for 50%, and particles with a particle size smaller than it also account for 50%.
[0041] In some embodiments of the present application, the specific surface area of the lithium-supplementing positive electrode material 100 is 3 m 2 / g-20m 2In some specific embodiments, the specific surface area of the lithium-supplementing positive electrode material 100 may be, for example, 3 m 2 / g, 5m 2 / g, 6m 2 / g, 8m 2 / g, 10m 2 / g, 12m 2 / g, 14m 2 / g, 15m 2 / g, 16m 2 / g, 18m 2 / g, 20m 2 In some embodiments, the specific surface area of the lithium-supplementing positive electrode material 100 may be 5 m 2 / g-18m 2 / g. The present application controls the particle size of the active material core and the lithium supplement particles within a suitable range and thus controls the specific surface area of the lithium supplement positive electrode material within a suitable range, thereby further improving the stability of the lithium supplement positive electrode material and improving the cycle performance and service life of the battery.
[0042] In some other embodiments of the present application, the active material core 101 is LiNi x3 Co y3 Mn 1-x3-y3 O2 and / or LiNi x4 Co y4 Al 1-x4-y4 O2, the particle size of the active material core 101 is 0.4μm-50μm, and the particle size of the lithium supplement particle 102 is 0.01μm-10μm. In some specific embodiments, the particle size of the active material core 101 can be, for example, 0.4μm, 0.5μm, 1μm, 2μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm; the particle size of the lithium supplement particles 102 can be, for example, 0.01μm, 0.02μm, 0.04μm, 0.05μm, 0.08μm, 0.1μm, 0.2μm, 0.4μm, 0.5μm, 0.8μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 5μm, 6μm, 8μm, 10μm. In some embodiments, the particle size of the active material core 101 can be 0.5 μm-20 μm, and the particle size of the lithium supplement particle 102 can be 0.02 μm-4 μm. When the active material is a ternary layered oxide type positive electrode material, controlling the particle size of the active material core and the lithium supplement particle within the above range is not only beneficial to the processing of the lithium supplement positive electrode material particles, but also beneficial to improving the processing stability of the slurry during the preparation of the slurry, thereby further improving the specific capacity and rate performance of the lithium supplement positive electrode material and further reducing the decomposition voltage.
[0043] In some embodiments of the present application, the specific surface area of the lithium-supplementing positive electrode material 100 is 0.2 m 2 / g-2m 2 In some specific embodiments, the specific surface area of the lithium-supplementing positive electrode material 100 may be, for example, 0.2 m 2 / g, 0.3m 2 / g, 0.5m 2 / g, 0.6m 2 / g, 0.8m 2 / g, 1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.8m 2 / g, 2m 2 In some embodiments, the specific surface area of the lithium-supplementing positive electrode material 100 may be 0.5 m 2 / g-1.5m 2 / g. The present application controls the particle size of the active material core and the lithium supplement particles within a suitable range and thus controls the specific surface area of the lithium supplement positive electrode material within a suitable range, thereby further improving the stability of the lithium supplement positive electrode material and improving the cycle performance and service life of the battery.
[0044] The lithium-supplemented positive electrode material provided in the present application can effectively avoid the gelation of the positive electrode active slurry and improve the electronic and ion conductivity of the lithium-supplemented positive electrode material by specially designing its structure, in-situ compounding of the lithium-supplemented particles with the active material core and coating with carbon. In addition, the structure of the lithium-supplemented positive electrode material can also effectively reduce the decomposition voltage, thereby solving the gas production problem of the battery during later use, thereby improving the battery's cycle performance, service life and safety performance.
[0045] The present application also provides a method for preparing the lithium-supplemented positive electrode material provided above, comprising:
[0046] S101, mixing a lithium source, a phosphorus source, an iron source and a carbon source to obtain a lithium-supplementing positive electrode material precursor; or, mixing a lithium source, a phosphorus source, an iron source, a manganese source and a carbon source to obtain a lithium-supplementing positive electrode material precursor;
[0047] S102, sintering the lithium-supplementing positive electrode material precursor to obtain a lithium-supplementing positive electrode material;
[0048] Or, include:
[0049] S201, mixing a lithium source, a nickel source, a cobalt source, and a manganese source or an aluminum source to obtain a lithium-supplementing positive electrode material precursor;
[0050] S202. Sinter the precursor of the lithium - supplemented cathode material, then mix it with a carbon source and perform a secondary sintering treatment to obtain the lithium - supplemented cathode material.
[0051] In step S101, the lithium source includes one or more of lithium carbonate, lithium hydroxide, lithium hydroxide monohydrate, lithium nitrate, lithium oxide, lithium peroxide, and lithium acetate; the phosphorus source includes one or more of lithium dihydrogen phosphate, iron phosphate, ammonium phosphate, sodium dihydrogen phosphate, lithium hydrogen phosphate, lithium phytate, and sodium tripolyphosphate; the iron source includes one or more of ferrous oxide, iron(III) oxide, iron nitrate, iron phosphate, ferrous oxalate, and ferrous sulfate; the carbon source includes one or several of sugars, polymer organic substances, and conductive carbon. Specifically, the carbon source includes one or more of glucose, sucrose, fructose, chitosan, lignin, carboxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, phenolic resin, needle coke, petroleum coke, pitch coke, pitch, polystyrene, poly(phenylacetylene), carbon black, acetylene black, super - P, carbon nanotubes, graphene, Ketjen black, and VGCF; one or more of manganese tetraoxide, manganese sulfate, manganese oxalate, manganese carbonate, manganese dioxide, and manganese acetate.
[0052] In some embodiments of the present application, the preparation raw materials of the precursor of the lithium - supplemented cathode material include a lithium source, a phosphorus source, an iron source, and a carbon source. The active material core of the prepared lithium - supplemented cathode material is Li x1 Fe y1 PO4, where 0.9 ≤ x1 ≤ 1.1 and 0.9 ≤ y1 ≤ 1.1. In the embodiments of the present application, the feeding ratio of the lithium source, the phosphorus source, the iron source, and the carbon source is (1 - 1.2):(0.9 - 1.1):(0.9 - 1.1):(0.02 - 0.1).
[0053] In other embodiments of the present application, the preparation raw materials of the precursor of the lithium - supplemented cathode material include a lithium source, a phosphorus source, an iron source, a carbon source, and a manganese source. The active material core of the prepared lithium - supplemented cathode material is LiFe x2 Mn 1-x2 PO4, where 0 < x2 < 1. In the embodiments of the present application, the feeding ratio of the lithium source, the phosphorus source, the iron source, the carbon source, and the manganese source is (1 - 1.2):(0.9 - 1.1):(0.4 - 0.6):(0.05 - 0.1):(0.4 - 0.6).
[0054] In the embodiments of the present application, the mixing method includes but is not limited to ball - milling mixing.
[0055] In step S102, the sintering treatment is carried out in a protective atmosphere, which includes but is not limited to a nitrogen atmosphere or an argon atmosphere. In the embodiments of the present application, the temperature of the sintering treatment is 600°C - 900°C, and the sintering time is 6h - 24h. The sintering temperature of the sintering treatment can be, for example, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C; the sintering time can be, for example, 6h, 8h, 10h, 12h, 15h, 16h, 20h, 24h. By controlling the temperature and time of the sintering treatment within a suitable range, the present application can obtain lithium iron phosphate type or lithium iron manganese phosphate type active material core particles, and on this basis, in-situ composite lithium supplement particles are formed. At this temperature, the carbon source plays a reducing role on the one hand and can also obtain a carbon coating layer on the surface of the lithium-supplemented cathode material on the other hand.
[0056] In step S201, the lithium source includes one or more of lithium carbonate, lithium hydroxide, lithium hydroxide monohydrate, lithium nitrate, lithium oxide, lithium peroxide, and lithium acetate; the nickel source includes one or more of nickel oxides, hydroxides, sulfates, and acetates; the cobalt source includes one or more of cobalt oxides, hydroxides, sulfates, and acetates; the manganese source includes one or more of manganese oxides, hydroxides, sulfates, and acetates; the aluminum source includes one or more of Al2O3, Al(OH)3, Al2(SO4)3, and Al(NO3)3.
[0057] In some embodiments of the present application, the raw materials for preparing the lithium-supplemented cathode material precursor include a lithium source, a nickel source, a cobalt source, and a manganese source. The active material core of the prepared lithium-supplemented cathode material is LiNi x3 Co y3 Mn 1-x3-y3 O2, 0 < x3 < 1, 0 < y3 < 1. In the embodiments of the present application, the feeding ratio of the lithium source, nickel source, cobalt source, and manganese source is (1 - 1.2):(0.1 - 0.5):(0.1 - 0.5):(0.1 - 0.5).
[0058] In other embodiments of the present application, the raw materials for preparing the lithium-supplemented cathode material precursor include a lithium source, a nickel source, a cobalt source, and an aluminum source. The active material core of the prepared lithium-supplemented cathode material is LiNi x4 Co y4 Al 1-x4-y4 O2, 0 < x4 < 1, 0 < y4 < 1. In the embodiments of the present application, the feeding ratio of the lithium source, nickel source, cobalt source, and aluminum source is (1 - 1.2):(0.1 - 0.5):(0.1 - 0.5):(0.1 - 0.5).
[0059] In the embodiments of the present application, the mixing method includes but is not limited to mixing by ball milling. The ball milling mixing time is 1h-12h. In some specific embodiments, the ball milling mixing time can be, for example, 1h, 2h, 3h, 5h, 10h, 12h.
[0060] In step S202, the sintering treatment is carried out under an oxygen or air atmosphere. In the embodiment of the present application, the temperature of the sintering treatment is 600°C-900°C, and the sintering time is 6h-24h. In some specific embodiments, the sintering temperature of the sintering treatment can be, for example, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C; the sintering time can be, for example, 6h, 8h, 10h, 12h, 15h, 16h, 20h, 24h. The present application can achieve the formation and growth of ternary layered oxide type positive electrode material crystals by controlling the temperature and time of the sintering treatment within a suitable range.
[0061] In the embodiment of the present application, the secondary sintering treatment is carried out under a protective atmosphere, and the protective atmosphere includes but is not limited to a nitrogen atmosphere or an argon atmosphere. In the embodiment of the present application, the temperature of the secondary sintering treatment is 700°C-1000°C, and the sintering time is 2h-8h. In some specific embodiments, the temperature of the secondary sintering treatment can be, for example, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, and the sintering time can be, for example, 2h, 3h, 4h, 5h, 6h, 7h, 8h. The present application adds a carbon source during the secondary sintering treatment and controls its temperature and time within a suitable range, so that the carbon source can be carbonized and a carbon coating layer can be obtained on the surface of the lithium-supplemented positive electrode.
[0062] The preparation method of the lithium-replenishing positive electrode material provided in the present application controls the feed ratio of each raw material within a suitable range to obtain a lithium-replenishing positive electrode material in which the active material core is in situ composited with lithium-replenishing particles and coated with carbon. The size of the lithium-replenishing particles of the lithium-replenishing positive electrode material is much smaller than that of a conventional lithium-replenishing agent. The prepared lithium-replenishing positive electrode material has no metal oxide residue after lithium replenishment, has lower requirements for the feed and coating process of the positive electrode preparation, and is not prone to gelation during the preparation of the slurry, thereby shortening the preparation process, reducing production costs and improving the preparation yield.
[0063] The present application also provides a positive electrode sheet, which includes a current collector and a positive electrode active layer loaded on the current collector, and the positive electrode active layer includes a lithium-supplementing positive electrode material as provided in the previous text of the present application or a lithium-supplementing positive electrode material prepared by the preparation method as provided in the previous text of the present application. In the embodiment of the present application, the positive electrode active layer also includes a binder and a conductive agent. In the embodiment of the present application, the conductive agent can be any conductive agent known in the art, including but not limited to one or more of super P-Li, superP, acetylene black, graphene and carbon nanotubes. In the embodiment of the present application, the binder can be any binder known in the art, including but not limited to polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyethylene oxide (PEO) and polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and the like.
[0064] The present application also provides a lithium-ion battery, which includes a positive electrode sheet, a negative electrode sheet, and a separator and an electrolyte located between the positive electrode sheet and the negative electrode sheet, and the positive electrode sheet includes a positive electrode sheet as provided in the previous text of the present application. In the embodiment of the present application, the separator includes but is not limited to a polymer film. In the embodiment of the present application, the negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on the negative electrode current collector, and the negative electrode active material in the negative electrode material layer can be any negative electrode active material for lithium-ion batteries known in the art. In the embodiment of the present application, the negative electrode active material in the negative electrode material layer can be any negative electrode active material for lithium-ion batteries known in the art. Exemplarily, the negative electrode active material can be selected from one or more of carbon-based negative electrode active materials, silicon-based negative electrode active materials, tin-based negative electrode active materials, and lithium metal negative electrode active materials. Among them, the carbon-based negative electrode includes but is not limited to natural graphite, artificial graphite, hard carbon, soft carbon, and graphene; the silicon-based negative electrode includes but is not limited to silicon, silicon carbon, silicon oxygen, etc.; the tin-based negative electrode includes but is not limited to tin, tin carbon, tin oxygen, and tin metal compounds.
[0065] The present application also provides an electrical device, which includes the lithium-ion battery described above. The electrical device may be, for example, an electric car, a mobile phone, a tablet computer, a laptop computer, a wearable device (a watch, a bracelet), a digital camera, etc.
[0066] The present application is further described below in multiple embodiments:
[0067] Example 1
[0068] Weigh lithium carbonate and iron phosphate in a molar ratio of 1.01:2 and sinter at 650° C. for 12 h to obtain a lithium iron phosphate intermediate;
[0069] Then, lithium iron phosphate intermediate, lithium carbonate and glucose in a molar ratio of 1:0.03:0.03 were weighed, ball-milled and mixed for 3 hours, and then sintered at 850° C. for 4 hours to obtain a lithium-supplementing positive electrode material;
[0070] The prepared lithium-replenishing positive electrode material is dissolved in N-methylpyrrolidone solvent to prepare positive electrode slurry, and the obtained positive electrode slurry is evenly coated on aluminum foil and vacuum dried to obtain a lithium-replenishing positive electrode sheet.
[0071] Example 2
[0072] Weigh lithium carbonate, iron phosphate and lithium manganate in a molar ratio of 1.01:0.8:1.2 and sinter at 650° C. for 12 h to obtain a lithium iron manganese phosphate intermediate;
[0073] Then, lithium manganese iron phosphate intermediate, lithium carbonate and glucose in a molar ratio of 1:0.03:0.03 were weighed, ball-milled and mixed for 3 hours, and then sintered at 850° C. for 4 hours to obtain a lithium-supplemented positive electrode material;
[0074] The prepared lithium-replenishing positive electrode material is dissolved in N-methylpyrrolidone solvent to prepare positive electrode slurry, and the obtained positive electrode slurry is evenly coated on aluminum foil and vacuum dried to obtain a lithium-replenishing positive electrode sheet.
[0075] Example 3
[0076] NiSO4·H2O, CoSO4·H2O, and MnSO4·H2O in a molar ratio of 5:2:3 were weighed and dissolved in a mixed solution of sodium hydroxide and ammonia water to obtain the ternary material intermediate Ni 0.5 Co 0.2 Mn 0.3 (OH)2;
[0077] Then weigh the ternary material intermediate Ni with a molar ratio of 2:1.05 0.5 Co 0.2 Mn 0.3 (OH)2 and lithium carbonate were sintered at 850℃ for 9h to obtain the active material core intermediate LiNi 0.5 Co 0.2 Mn 0.3 O2;
[0078] Then weigh lithium carbonate and LiNi in a molar ratio of 1:0.03:0.02. 0.5 Co 0.2 Mn 0.3 O2 and glucose were ball-milled for 3 hours and then sintered at 950°C for 4 hours to obtain a lithium-supplementing positive electrode material;
[0079] The prepared lithium-replenishing positive electrode material is dissolved in N-methylpyrrolidone solvent to prepare positive electrode slurry, and the obtained positive electrode slurry is evenly coated on aluminum foil and vacuum dried to obtain a lithium-replenishing positive electrode sheet.
[0080] Example 4
[0081] Weigh lithium carbonate and iron phosphate in a molar ratio of 1.01:2 and sinter at 650° C. for 12 h to obtain a lithium iron phosphate intermediate;
[0082] Then, lithium iron phosphate intermediate, Li2C4O4 and glucose were weighed in a molar ratio of 1:0.03:0.03, ball-milled and mixed for 3 hours, and then sintered at 850°C for 4 hours to obtain a lithium-supplemented positive electrode material;
[0083] The prepared lithium-replenishing positive electrode material is dissolved in N-methylpyrrolidone solvent to prepare positive electrode slurry, and the obtained positive electrode slurry is evenly coated on aluminum foil and vacuum dried to obtain a lithium-replenishing positive electrode sheet.
[0084] Example 5
[0085] Weigh lithium carbonate and iron phosphate in a molar ratio of 1.01:2 and sinter at 650° C. for 12 h to obtain a lithium iron phosphate intermediate;
[0086] Then, lithium iron phosphate intermediate, lithium carbonate and glucose in a molar ratio of 1:0.06:0.03 were weighed, ball-milled and mixed for 3 hours, and then sintered at 850° C. for 4 hours to obtain a lithium-supplemented positive electrode material;
[0087] The prepared lithium-replenishing positive electrode material is dissolved in N-methylpyrrolidone solvent to prepare positive electrode slurry, and the obtained positive electrode slurry is evenly coated on aluminum foil and vacuum dried to obtain a lithium-replenishing positive electrode sheet.
[0088] Example 6
[0089] Weigh lithium carbonate and iron phosphate in a molar ratio of 1.01:2 and sinter at 650° C. for 12 h to obtain a lithium iron phosphate intermediate;
[0090] Then, lithium iron phosphate intermediate, lithium carbonate and glucose in a molar ratio of 1:0.02:0.03 were weighed, ball-milled and mixed for 3 hours, and then sintered at 850° C. for 4 hours to obtain a lithium-supplementing positive electrode material;
[0091] The prepared lithium-replenishing positive electrode material is dissolved in N-methylpyrrolidone solvent to prepare positive electrode slurry, and the obtained positive electrode slurry is evenly coated on aluminum foil and vacuum dried to obtain a lithium-replenishing positive electrode sheet.
[0092] Example 7
[0093] Weigh lithium carbonate and iron phosphate in a molar ratio of 1.01:2 and sinter at 650° C. for 12 h to obtain a lithium iron phosphate intermediate;
[0094] Then, lithium iron phosphate intermediate, lithium carbonate and glucose in a molar ratio of 1:0.03:0.03 were weighed, ball-milled and mixed for 7 hours, and then sintered at 850° C. for 4 hours to obtain a lithium-supplemented positive electrode material;
[0095] The prepared lithium-replenishing positive electrode material is dissolved in N-methylpyrrolidone solvent to prepare positive electrode slurry, and the obtained positive electrode slurry is evenly coated on aluminum foil and vacuum dried to obtain a lithium-replenishing positive electrode sheet.
[0096] Comparative Example 1
[0097] Weigh 100 parts by weight of active material lithium iron phosphate and dissolve it in N-methylpyrrolidone solvent to prepare lithium iron phosphate slurry, then weigh 1.4 parts by weight of lithium supplement agent Li2CO3 and add it to the lithium iron phosphate slurry, stir evenly to obtain positive electrode slurry, evenly apply the obtained positive electrode slurry on aluminum foil and vacuum dry it to obtain a lithium supplement positive electrode sheet.
[0098] Performance Testing
[0099] Specific surface area: The lithium-supplemented positive electrode materials of Examples 1 to 7 were tested according to the national standard "Determination of Specific Surface Area of Solid Materials by Gas Adsorption BET Method" (GB / T 19587-2017) to measure their specific surface areas. The results are shown in Table 1.
[0100] Particle size D50: The particle sizes of the active material cores and lithium-supplementing particles of Examples 1 to 7 and the lithium-supplementing particles of Comparative Example 1 were tested using a laser particle size distribution analyzer. The measured particle sizes D50 are shown in Table 1.
[0101] The lithium-supplemented positive electrode plates and negative electrodes, separators, and electrolytes prepared in Examples 1 to 7 and Comparative Example 1 are converted into soft-pack batteries.
[0102] Gas production performance: The SOC of the soft-pack batteries prepared in Examples 1 to 7 and Comparative Example 1 was adjusted to 100%, 90%, 80%, 70%, 60%, 50%, 40%, 30%, 20%, 10%, and 0% in turn. After being stored at 60°C for 28 days, the battery weight was tested by the drainage method. The gas production performance of the battery was calculated and statistically analyzed by the weight difference. The results are shown in Table 1.
[0103] Cycle performance: The soft-pack batteries prepared in Examples 1 to 7 and Comparative Example 1 were charged at 45°C with a cutoff current of 0.05C from 0.5CCC-CV to 3.7V and discharged at 0.5C to 2.3V. After 1000 cycles, the retention rate of the battery capacity relative to the battery capacity before the cycle was checked. The results are shown in Table 1.
[0104] Rate performance: The soft-pack batteries prepared in Examples 1 to 7 and Comparative Example 1 were charged at 25°C with a cutoff current of 0.05C from 0.5C CC-CV to 3.7V and discharged at 0.1C to 2.3V, and the capacity was recorded as C1; at 25°C, the cutoff current of 0.05C from 0.5C CC-CV to 3.7V and discharged at 2C to 2.3V were recorded as C2; the calculation formula for the 2C / 0.1C capacity retention rate was: C2 / C1*100%, and the results are shown in Table 1.
[0105] Table 1
[0106]
[0107] It can be seen from Table 1 that compared with Comparative Example 1 in which lithium-replenishing particles are directly added to the active slurry, Examples 1 to 7 of the present application significantly reduce the particle size of the lithium-replenishing particles by in-situ composite lithium-replenishing particles in the core of the positive electrode active material and coating them with carbon materials, effectively reduce the risk of gelation of the positive electrode active slurry caused by residual alkali on the surface of the lithium-replenishing particles, and can improve the electronic conductivity and ion conductivity of the lithium-replenishing positive electrode material, and also reduce its decomposition starting voltage, increase the decomposition rate, reduce the gas production of the battery, and thereby improve the cycle performance and rate performance of the battery.
[0108] The preferred embodiments are described in detail above, but the present invention is not limited to the above-mentioned specific implementation modes. Under the guidance of the present application, technicians in this field can also make various specific changes without departing from the scope of protection of the present application, which all fall within the scope of protection of the present invention.
Claims
1. A lithium-supplementing positive electrode material, characterized in that: The lithium - supplemented cathode material includes an active material core and a coating layer coated on the surface of the active material core. The coating layer includes lithium - supplemented particles and carbon; the active material core includes Li x1 Fe y1 PO4, LiFe x2 Mn 1-x2 PO4, LiNi x3 Co y3 Mn 1-x3-y3 O2 and LiNi x4 Co y4 Al 1-x4-y4 O2, one or more of them, where 0.9 ≤ x1 ≤ 1.1, 0.9 ≤ y1 ≤ 1.1, 0 < x2 < 1, 0 < x3 < 1, 0 < y3 < 1, 0 < x4 < 1, 0 < y4 < 1; the lithium - supplemented particles include Li a C b O c , where 0 < a ≤ 6, 0 < b ≤ 6, 0 < c ≤ 6.
2. The lithium-supplementing positive electrode material according to claim 1, characterized in that: The carbon is coated on the surface of the active material core and / or the surface of the lithium supplement particle.
3. The lithium-supplementing positive electrode material according to claim 1 or 2, characterized in that: At least part of the lithium-supplementing particles are in-situ grown on the surface of the active material core.
4. The lithium-supplementing positive electrode material according to any one of claims 1 to 3, characterized in that: The lithium supplement particles include one or more of Li2C4O4, Li2CO3, Li2C2O4 and Li6C6O6.
5. The lithium-supplementing positive electrode material according to any one of claims 1 to 4, characterized in that: The mass ratio of the lithium supplement particles to the active material core is (0.1-10):
100.
6. The lithium-supplementing positive electrode material according to any one of claims 1 to 5, characterized in that: The mass percentage of the carbon in the lithium-supplementing positive electrode material is 0.1%-5%.
7. The lithium-supplementing positive electrode material according to any one of claims 1 to 6, characterized in that: The particle size of the active material core is 0.02 μm-50 μm; the particle size of the lithium supplement particle is 0.01 μm-10 μm.
8. The lithium-supplemented positive electrode material according to claim 7, characterized in that: When the active material core is Li x1 Fe y1 PO4 and / or LiFe x2 Mn 1-x2 PO4, the particle size of the active material core is 0.02 μm-15 μm, and the particle size of the lithium supplement particles is 0.01 μm-8 μm; when the active material core is LiNi x3 Co y3 Mn 1-x3-y3 O2 and / or LiNi x4 Co y4 Al 1-x4-y4 When O2 is used, the particle size of the active material core is 0.4 μm-50 μm, and the particle size of the lithium supplement particle is 0.01 μm-10 μm.
9. The lithium-supplementing positive electrode material according to any one of claims 1 to 8, characterized in that: The specific surface area of the lithium-supplementing positive electrode material is 0.2 m 2 / g-20m 2 / g.
10. A method for preparing the lithium-supplemented positive electrode material according to any one of claims 1 to 9, characterized in that: include: Mixing a lithium source, a phosphorus source, an iron source and a carbon source to obtain a lithium-supplementing positive electrode material precursor; or, mixing a lithium source, a phosphorus source, an iron source, a manganese source and a carbon source to obtain a lithium-supplementing positive electrode material precursor; Sintering the lithium-supplementing positive electrode material precursor to obtain a lithium-supplementing positive electrode material; Or, include: Mixing a lithium source, a nickel source, a cobalt source, and a manganese source or an aluminum source to obtain a lithium-supplemented positive electrode material precursor; The lithium-replenishing positive electrode material precursor is sintered, and then mixed with a carbon source and subjected to secondary sintering to obtain the lithium-replenishing positive electrode material.
11. The method for preparing a lithium-supplemented positive electrode material according to claim 10, characterized in that: The temperature of the sintering treatment is 600°C-900°C, and the sintering time is 6h-24h; the temperature of the secondary sintering treatment is 700°C-1000°C, and the sintering time is 2h-8h.
12. A positive electrode sheet, characterized in that: The positive electrode sheet includes a current collector and a positive electrode active layer loaded on the current collector, and the positive electrode active layer includes the lithium-supplementing positive electrode material according to any one of claims 1 to 9 or the lithium-supplementing positive electrode material prepared by the preparation method according to any one of claims 10 to 11.
13. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 12.
14. An electrical device, characterized in that: The electrical device comprises the lithium-ion battery as claimed in claim 13.
Citation Information
Cited By
Coated lithium supplement material, preparation method and application thereof, and lithium ion battery
CN119812243A
High-rate lithium ferric manganese phosphate material as well as preparation method and application thereof
CN120504304A
Prelithiated positive electrode material, and preparation method therefor and use thereof
WO2026065927A1
Lithium-supplementing positive electrode material, and preparation method therefor and use thereof
WO2026065928A1