Anti-adhesion CPP film for lithium battery packaging aluminum plastic film and preparation method of anti-adhesion CPP film
By using a multi-layer structure of anti-adhesion CPP film in lithium battery encapsulated aluminum-plastic film, the adhesion during high-temperature baking is solved by using maleic anhydride grafted polypropylene, random copolymer polypropylene and modified silica. The problem has improved the performance and safety of lithium batteries, shortened the water removal time, and improved production efficiency.
Patent Information
- Application Number
- CN202411122301.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-29
AI Technical Summary
The existing lithium battery-encapsulated aluminum-plastic films are prone to stick to each other during high temperature baking, which affects battery performance and safety, and slow moisture removal speed, affects production efficiency.
Anti-adhesion CPP film designed with a multi-layer structure, including composite layer, core layer and heat sealing layer, using maleic anhydride grafted polypropylene, random copolymer polypropylene, modified silica and acrylate materials, through modification The surface treatment and polymerization of silica improve the film's high temperature resistance and anti-static properties.
It significantly improves the film's high-temperature baking and anti-static properties, reduces the adhesion and wrinkle phenomenon during maturation of aluminum-plastic film, shortens the water removal time of the battery cell preparation process, and improves the packaging efficiency and performance of lithium battery.
Smart Images

Figure BDA0004995433740000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging materials, and in particular to an anti-adhesion CPP film for lithium battery packaging aluminum-plastic film and a preparation method thereof. Background Art
[0002] Since the industrialization of lithium-ion batteries in the early 1990s, they have become the battery system with the best comprehensive performance and are widely used in the civilian field, such as mobile phones, PDAs, laptops, camcorders, digital cameras, etc., due to their small size, light weight, long cycle life (more than 1,000 times), no memory effect (can be charged at any time without affecting performance), high discharge voltage (discharge voltage is 3 times that of nickel-cadmium and nickel-metal hydride batteries), and green environmental protection. At the same time, with the development of lithium-ion battery technology, the application field of lithium-ion batteries has gradually expanded, and large-capacity lithium-ion batteries that can be used in electric vehicles, aerospace and energy storage are also being accelerated.
[0003] Lithium-ion battery aluminum-plastic composite film soft packaging is a composite soft packaging material composed of aluminum foil, various plastics and various adhesives (including adhesive resins). This aluminum-plastic composite film soft packaging plays an important role in protecting lithium-ion battery fluid and acting as a shell material. It forms a battery core together with the battery fluid, and the battery core is assembled to form a lithium-ion battery. Generally speaking, the basic composition of aluminum-plastic composite film soft packaging can be divided into inner layer / middle layer / outer layer.
[0004] The key barrier in the aluminum-plastic composite film soft packaging material for lithium batteries is the middle layer - the aluminum foil layer. The outer layer mainly protects the middle aluminum foil layer and is suitable for the processing requirements of cold stamping formability. In particular, it also requires good printability, and PET is usually selected. The inner multifunctional layer is a composite layer and heat-sealing layer with chemical stability designed and manufactured for the special properties of the electrolyte in lithium-ion batteries. The materials used in the inner layer are usually PP (polypropylene), PE (polyethylene), EAA (ethylene-acrylic acid copolymer), CPP (polypropylene or modified polypropylene) or ion cross-linked polymer resin and other film materials. These materials have been repeatedly studied and verified at home and abroad and can be used as inner layer materials for lithium-ion battery packaging. These materials generally have good heat sealing properties, and they are polyolefin materials with certain chemical corrosion resistance. They do not react with electrolytes and have strong acid resistance, which can improve the electrolyte resistance of packaging materials. According to product requirements, the inner film material can be compounded with the aluminum foil layer using single-layer casting, hot pressing or multi-layer co-extrusion production processes. No matter which process is used, the multifunctional layer used as the inner material must have good thermal adhesion with the aluminum foil, good self-heat sealing ability with tabs, moderate strength, excellent moisture resistance and heat resistance, and good chemical resistance when in contact with the electrolyte, so as to ensure the performance of the final battery and a longer service life.
[0005] Chinese patent document CN112918054A discloses a CPP for aluminum-plastic film and a production method thereof, comprising an A layer, a B layer and a C layer, wherein the A layer comprises 79.5 to 89 parts by mass of random copolymer polypropylene, 5 to 7 parts by mass of an organic boron nonionic active agent, 0.5 to 1 parts by mass of a toughening agent, 1 to 3 parts by mass of an adhesion promoter, 2 to 5 parts by mass of a light shielding agent, 5 to 10 parts by mass of graphene powder and 2 to 5 parts by mass of an anti-aging agent.
[0006] During the production process of the battery cell, a certain amount of moisture will be introduced. If the moisture is not controlled within the standard in time, it will seriously affect the performance and safety of the battery. After the soft-pack battery is sealed on the top / side and the parallelism of the core is checked, the moisture is removed by baking in a vacuum environment and with the action of a desiccant. The existing heating temperature is generally 85°C for more than 24 hours. If the baking temperature is increased to above 100°C, the removal of moisture can be accelerated. At this time, the CPP is in contact under the action of a vacuum. Due to the insufficient temperature resistance of the existing CPP, adhesion usually occurs after the baking temperature is increased, affecting the subsequent liquid injection process. Summary of the invention
[0007] In order to solve the deficiencies in the prior art, the purpose of the present invention is to provide an anti-sticking CPP film for lithium battery encapsulation aluminum-plastic film and a preparation method thereof. Through multi-layer structure design and material formulation, the CPP film can withstand high-temperature baking above 100°C, effectively solving the problem that the existing CPP is easy to stick at high temperatures, not only speeding up the removal of moisture inside the battery, shortening the baking time, and improving production efficiency, but also better controlling the moisture content inside the battery, thereby improving the performance and safety of the battery.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] An anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film, comprising a composite layer, a core layer and a heat-sealing layer stacked in sequence;
[0010] Preferably, the composite layer is made of the following components in parts by weight: 30-40 parts of maleic anhydride grafted polypropylene, 40-50 parts of random copolymerized polypropylene, 5-10 parts of EVA, 10-20 parts of modified silica, and 5-8 parts of acrylate.
[0011] More preferably, the composite layer is made of the following components in parts by weight: 35 parts of maleic anhydride grafted polypropylene, 45 parts of random copolymerized polypropylene, 7.5 parts of EVA, 20 parts of modified silica, and 6.5 parts of acrylate.
[0012] Preferably, the core layer is made of the following components in parts by weight: 45-65 parts of block copolymer polypropylene, 10-30 parts of POE, and 15-30 parts of terpolymer polypropylene;
[0013] More preferably, the core layer is made of the following components in parts by weight: 50 parts of block copolymer polypropylene, 20 parts of POE, and 22 parts of terpolymer polypropylene;
[0014] Preferably, the heat-sealing layer is made of the following components in parts by weight: 50-70 parts of binary copolymer polypropylene, 10-20 parts of POE, and 5-20 parts of homopolymer polypropylene.
[0015] More preferably, the heat-sealing layer is made of the following components in parts by weight: 60 parts of binary copolymer polypropylene, 15 parts of POE, and 12 parts of homopolymer polypropylene.
[0016] Preferably, the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C.
[0017] Preferably, the total thickness of the CPP film is 20-100 μm; the thickness of the composite layer is 10%-30% of the total thickness of the CPP film; and the thickness of the heat-sealing layer is 10%-30% of the total thickness of the CPP film.
[0018] Preferably, the method for preparing the modified silicon dioxide comprises the following steps:
[0019] (1) dispersing silica into an ethanol / water mixture, then adding KH570, stirring for reaction, filtering, washing, and drying the product to obtain olefinated silica;
[0020] (2) dispersing olefinated silica in tetrahydrofuran, then adding methacryloyloxyethyl trimethylammonium chloride, allyl acrylate, and oleyl palmitamide, ultrasonically treating, slowly adding dibenzoyl peroxide under stirring, polymerizing under a nitrogen atmosphere, precipitating the product with anhydrous ether, washing with alcohol, and drying to obtain the modified silica.
[0021] Preferably, in step (1), the ethanol / water mixture is obtained by mixing anhydrous ethanol and deionized water in a volume ratio of 10:4-8, and the amount ratio of silicon dioxide, ethanol / water mixture and KH570 is 10g:100mL:1-5g.
[0022] Preferably, in step (1), the stirring reaction condition is 50-65° C. for 1-4 h.
[0023] Specifically, in step (1), the stirring reaction temperature can be 50°C, 53°C, 56°C, 59°C, 62°C, or 65°C; and the stirring reaction time can be 1 h, 2 h, 3 h, or 4 h.
[0024] Preferably, in step (2), the ultrasonic treatment time is 20 to 40 minutes, and the polymerization reaction conditions are polymerization at 50 to 65° C. for 18 to 36 hours.
[0025] Specifically, in step (2), the ultrasonic treatment time can be 20 min, 25 min, 30 min, 35 min, 40 min; the polymerization reaction temperature can be 50°C, 55°C, 60°C, 65°C; the polymerization reaction time can be 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h, 34h, 36h.
[0026] Preferably, in step (2), the mass ratio of olefinated silica, methacryloyloxyethyl trimethylammonium chloride, allyl acrylate, and oleyl palmitamide is 10:2-12:0.5-3:2-12; and the amount of dibenzoyl peroxide is 0.1% to 1% of the total mass of the monomers.
[0027] The present invention also claims protection for a method for preparing the anti-adhesion CPP film for the lithium battery encapsulation aluminum-plastic film, comprising the following steps: melting the raw materials according to the formula through three single-screw extruders respectively, and then passing through a batching block connector, a die head for co-extrusion, and cast film formation. The product is subsequently cooled and shaped, thickness detected, online slitting, winding and packaging to obtain the anti-adhesion CPP film for the lithium battery encapsulation aluminum-plastic film.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) The present invention provides an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film, which is made of a composite layer, a core layer and a heat-sealing layer. The composite layer adopts maleic anhydride grafted polypropylene, random copolymerized polypropylene, EVA, modified silica and acrylate. The random copolymerized polypropylene has the characteristics of high toughness. Maleic anhydride grafted polypropylene has better compatibility with inorganic particles than polypropylene. The modified silica can give the CPP film excellent antistatic property, anti-adhesion property and mechanical strength, and can also significantly improve the high temperature baking performance of the film. The finally prepared CPP film has good impact resistance and mechanical strength, and also improves the antistatic ability and anti-adhesion performance, and can withstand high temperature baking, effectively reducing the adhesion, wrinkles and uneven force of the aluminum-plastic film during maturation, significantly shortening the dehydration time in the battery preparation process, and improving the lithium battery packaging efficiency.
[0030] 2) The present invention provides a modified silica. First, KH570 silane coupling agent is used to perform surface treatment on nano silica. Siloxane in KH570 is hydrolyzed to generate Si-OH, which undergoes dehydration condensation with hydroxyl groups on the surface of nano silica, and organic chains and unsaturated double bonds are introduced into the surface of nano silica, thereby significantly improving the compatibility of nano silica with polypropylene resin. Subsequently, methacryloyloxyethyl trimethyl ammonium chloride and oleyl palmitamide are grafted onto the surface of nano silica through free radical polymerization reaction using allyl acrylate as a crosslinking agent in an inert atmosphere. The introduced quaternary ammonium salt can absorb moisture in the atmosphere to form a conductive film on the surface of the material, thereby effectively preventing the generation and accumulation of static electricity and reducing the generation and accumulation of static electricity. The film is wrinkled and stuck together due to electricity; the introduced oil-based palmitamide itself is a lubricant, which can form a film on the surface of the CPP film, reduce the mutual adhesion between the films, reduce the friction coefficient of the film surface, and make the films easy to slide, thereby improving the opening; since static electricity is mostly distributed on the surface of the film, and oil-based palmitamide has the characteristic of migrating to the surface of the film, it can cooperate with quaternary ammonium salt to form a dense conductive path on the surface of the film and eliminate static electricity on the surface of the CPP film; and nano-silica can effectively avoid the problems of easy migration and precipitation of methacryloyloxyethyl trimethylammonium chloride and oil-based palmitamide, and poor durability, while also improving the impact resistance, mechanical properties and high temperature baking resistance of the matrix. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0032] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.
[0033] Silica particle size 30~100nm;
[0034] Maleic anhydride grafted polypropylene was purchased from Coase Chemical Co., Ltd., model B1A;
[0035] Homopolymer polypropylene was provided by Shanghai Jinshan Petrochemical Company, brand FC801;
[0036] The terpolymer polypropylene was provided by Singapore TPC Company, with the trade name FL7632L;
[0037] The binary copolymer polypropylene was provided by Samsung of South Korea, with the trade name RF402;
[0038] EVA was purchased from Shanghai Fuchen Plastic Raw Materials Co., Ltd., brand number Japan Mitsui 420;
[0039] POE was purchased from Mitsui Chemicals, brand DF840.
[0040] A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film comprises the following steps:
[0041] (1) dispersing 10 g of silica into 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:4-8), then adding 1-5 g of KH570, stirring and reacting at 50-65° C. for 1-4 h, filtering, washing, and drying the product to obtain olefinated silica;
[0042] (2) dispersing 10 g of olefinated silica into 200 mL of tetrahydrofuran, then adding 2-12 g of methacryloyloxyethyl trimethylammonium chloride, 0.5-3 g of allyl acrylate, and 2-12 g of oleyl palmitamide, ultrasonically treating for 20-40 min, condensing and refluxing, continuously introducing nitrogen, slowly adding dibenzoyl peroxide (the amount of dibenzoyl peroxide is 0.1% to 1% of the total weight of the monomer) under stirring, and polymerizing at 50-65° C. for 18-36 h. The product is precipitated with anhydrous ether, washed with alcohol, and dried to obtain the modified silica;
[0043] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The products are subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film with a thickness of 20 to 100 μm.
[0044] The composite layer is made of the following components in parts by weight: 30-40 parts of maleic anhydride grafted polypropylene, 40-50 parts of random copolymer polypropylene, 5-10 parts of EVA, 10-20 parts of modified silica, and 5-8 parts of acrylate; the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the thickness of the composite layer is 10%-30% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 45-65 parts of block copolymer polypropylene, POE The weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C; the heat sealing layer is made of the following components in parts by weight: 50-70 parts of binary copolymer polypropylene, 10-20 parts of POE, and 5-20 parts of homopolymer polypropylene; the thickness of the heat sealing layer is 10%-30% of the total thickness of the CPP film.
[0045] The present invention will be further described below through specific embodiments.
[0046] Example 1
[0047] A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film comprises the following steps:
[0048] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:8), and then 5 g of KH570 was added, and the mixture was stirred and reacted at 65° C. for 1 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0049] (2) 10 g of olefinated silica was dispersed in 200 mL of tetrahydrofuran, and then 12 g of methacryloyloxyethyl trimethylammonium chloride, 3 g of allyl acrylate, and 12 g of oleyl palmitamide were added, and ultrasonic treatment was performed for 40 min, condensed and refluxed, and nitrogen was continuously introduced. 0.25 g of dibenzoyl peroxide was slowly added under stirring, and the polymerization reaction was carried out at 65° C. for 18 h. The product was precipitated with anhydrous ether, washed with alcohol, and dried to obtain the modified silica;
[0050] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film with a thickness of 54 μm.
[0051] The composite layer is made of the following components in parts by weight: 35kg of maleic anhydride grafted polypropylene, 45kg of random copolymer polypropylene, 8kg of EVA, 20kg of modified silica, and 6.5kg of acrylate; the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the thickness of the composite layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 55kg of block copolymer polypropylene, 20kg of POE, and 25kg of ternary copolymer polypropylene; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C; the heat sealing layer is made of the following components in parts by weight: 60kg of binary copolymer polypropylene, 15kg of POE, and 12kg of homopolymer polypropylene; the thickness of the heat sealing layer is 30% of the total thickness of the CPP film.
[0052] Example 2
[0053] A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film comprises the following steps:
[0054] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:6), and then 4 g of KH570 was added, and the mixture was stirred and reacted at 60° C. for 2 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0055] (2) 10 g of olefinated silica was dispersed in 200 mL of tetrahydrofuran, and then 9 g of methacryloyloxyethyl trimethylammonium chloride, 2 g of allyl acrylate, and 9 g of oleyl palmitamide were added, and ultrasonic treatment was performed for 30 min, condensed and refluxed, and nitrogen was continuously introduced. 0.2 g of dibenzoyl peroxide was slowly added under stirring, and the polymerization reaction was carried out at 60° C. for 24 h. The product was precipitated with anhydrous ether, washed with alcohol, and dried to obtain the modified silica;
[0056] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film with a thickness of 58 μm.
[0057] The composite layer is made of the following components in parts by weight: 35kg of maleic anhydride grafted polypropylene, 45kg of random copolymer polypropylene, 8kg of EVA, 16kg of modified silica, and 6.5kg of acrylate; the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the thickness of the composite layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 55kg of block copolymer polypropylene, 20kg of POE, and 25kg of ternary copolymer polypropylene; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C; the heat sealing layer is made of the following components in parts by weight: 60kg of binary copolymer polypropylene, 15kg of POE, and 12kg of homopolymer polypropylene; the thickness of the heat sealing layer is 30% of the total thickness of the CPP film.
[0058] Example 3
[0059] A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film comprises the following steps:
[0060] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:6), and then 3 g of KH570 was added, and the mixture was stirred at 50-65° C. for 1-4 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0061] (2) 10 g of olefinated silica was dispersed in 200 mL of tetrahydrofuran, and then 6 g of methacryloyloxyethyl trimethylammonium chloride, 1 g of allyl acrylate, and 6 g of oleyl palmitamide were added, and ultrasonic treatment was performed for 30 min, condensed and refluxed, and nitrogen was continuously introduced. 0.1 g of dibenzoyl peroxide was slowly added under stirring, and the polymerization reaction was carried out at 55° C. for 30 h. The product was precipitated with anhydrous ether, washed with alcohol, and dried to obtain the modified silica;
[0062] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film with a thickness of 62 μm.
[0063] The composite layer is made of the following components in parts by weight: 35kg of maleic anhydride grafted polypropylene, 45kg of random copolymer polypropylene, 8kg of EVA, 13kg of modified silica, and 6.5kg of acrylate; the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the thickness of the composite layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 55kg of block copolymer polypropylene, 20kg of POE, and 25kg of ternary copolymer polypropylene; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C; the heat sealing layer is made of the following components in parts by weight: 60kg of binary copolymer polypropylene, 15kg of POE, and 12kg of homopolymer polypropylene; the thickness of the heat sealing layer is 30% of the total thickness of the CPP film.
[0064] Example 4
[0065] A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film comprises the following steps:
[0066] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:4), and then 1 g of KH570 was added, and the mixture was stirred at 50° C. for 4 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0067] (2) 10 g of olefinated silica was dispersed in 200 mL of tetrahydrofuran, and then 2 g of methacryloyloxyethyl trimethylammonium chloride, 0.5 g of allyl acrylate, and 2 g of oleyl palmitamide were added, and ultrasonic treatment was performed for 20 min, condensed and refluxed, and nitrogen was continuously introduced. 0.05 g of dibenzoyl peroxide was slowly added under stirring, and the polymerization reaction was carried out at 50° C. for 36 h. The product was precipitated with anhydrous ether, washed with alcohol, and dried to obtain the modified silica;
[0068] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film with a thickness of 58 μm.
[0069] The composite layer is made of the following components in parts by weight: 35kg of maleic anhydride grafted polypropylene, 45kg of random copolymer polypropylene, 8kg of EVA, 10kg of modified silica, and 6.5kg of acrylate; the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the thickness of the composite layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 55kg of block copolymer polypropylene, 20kg of POE, and 25kg of ternary copolymer polypropylene; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C; the heat sealing layer is made of the following components in parts by weight: 60kg of binary copolymer polypropylene, 15kg of POE, and 12kg of homopolymer polypropylene; the thickness of the heat sealing layer is 30% of the total thickness of the CPP film.
[0070] Comparative Example 1
[0071] A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film comprises the following steps:
[0072] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:8), and then 5 g of KH570 was added, and the mixture was stirred and reacted at 65° C. for 1 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0073] (2) 10 g of olefinated silica was dispersed in 200 mL of tetrahydrofuran, and then 12 g of methacryloyloxyethyl trimethylammonium chloride and 3 g of allyl acrylate were added, and ultrasonic treatment was performed for 40 min, condensed and refluxed, and nitrogen was continuously introduced. 0.25 g of dibenzoyl peroxide was slowly added under stirring, and the polymerization reaction was carried out at 65° C. for 18 h. The product was precipitated with anhydrous ether, washed with alcohol, and dried to obtain the modified silica;
[0074] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film with a thickness of 56 μm.
[0075] The composite layer is made of the following components in parts by weight: 35kg of maleic anhydride grafted polypropylene, 45kg of random copolymer polypropylene, 8kg of EVA, 20kg of modified silica, and 6.5kg of acrylate; the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the thickness of the composite layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 55kg of block copolymer polypropylene, 20kg of POE, and 25kg of ternary copolymer polypropylene; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C; the heat sealing layer is made of the following components in parts by weight: 60kg of binary copolymer polypropylene, 15kg of POE, and 12kg of homopolymer polypropylene; the thickness of the heat sealing layer is 30% of the total thickness of the CPP film.
[0076] Comparative Example 2
[0077] A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film comprises the following steps:
[0078] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:8), and then 5 g of KH570 was added, and the mixture was stirred and reacted at 65° C. for 1 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0079] (2) 10 g of olefinated silica was dispersed in 200 mL of tetrahydrofuran, and then 3 g of allyl acrylate and 12 g of oleyl palmitamide were added, and ultrasonic treatment was performed for 40 min, condensed and refluxed, and nitrogen was continuously introduced. 0.25 g of dibenzoyl peroxide was slowly added under stirring, and the polymerization reaction was carried out at 65° C. for 18 h. The product was precipitated with anhydrous ether, washed with alcohol, and dried to obtain the modified silica;
[0080] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film with a thickness of 54 μm.
[0081] The composite layer is made of the following components in parts by weight: 35kg of maleic anhydride grafted polypropylene, 45kg of random copolymer polypropylene, 8kg of EVA, 20kg of modified silica, and 6.5kg of acrylate; the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the thickness of the composite layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 55kg of block copolymer polypropylene, 20kg of POE, and 25kg of ternary copolymer polypropylene; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C; the heat sealing layer is made of the following components in parts by weight: 60kg of binary copolymer polypropylene, 15kg of POE, and 12kg of homopolymer polypropylene; the thickness of the heat sealing layer is 30% of the total thickness of the CPP film.
[0082] Comparative Example 3
[0083] A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film comprises the following steps:
[0084] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:8), and then 5 g of KH570 was added, and the mixture was stirred and reacted at 65° C. for 1 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0085] (2) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film with a thickness of 57 μm.
[0086] The composite layer is made of the following components in parts by weight: 35kg of maleic anhydride grafted polypropylene, 45kg of random copolymer polypropylene, 8kg of EVA, 20kg of modified silica, and 6.5kg of acrylate; the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the thickness of the composite layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 55kg of block copolymer polypropylene, 20kg of POE, and 25kg of ternary copolymer polypropylene; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C; the heat sealing layer is made of the following components in parts by weight: 60kg of binary copolymer polypropylene, 15kg of POE, and 12kg of homopolymer polypropylene; the thickness of the heat sealing layer is 30% of the total thickness of the CPP film.
[0087] The CPP films prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to performance tests. The tensile strength and elongation at break were tested with reference to GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets"; the sample was aged and cut into 2.5 cm × 10 cm strips, laminated with aluminum foil, placed in a 100 ° C oven for 4 h, and then cooled for 2 h. The sample was peeled off at a peeling speed (300 mm / min) in the 180 ° direction using a peeling force machine (Kejian, KJ-1065A-H), and the heat-resistant adhesive force (g / 25 mm) was tested with reference to GB / T 2792-2014 "Test method for peel strength of adhesive tape"; the heat-resistant adhesive force (g / 25 mm) was tested with reference to GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics" to test light transmittance and haze; GB / T10006-2021 "Determination of friction coefficient of plastic films and sheets" to test dynamic friction coefficient; GB / T 31838.4-2019 "Dielectric and resistance properties of solid insulating materials Part 4: Resistance properties (DC method) Insulation resistance" to test surface resistance. Specific data are shown in Table 1.
[0088] Table 1 CPP film performance test results
[0089]
[0090] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film, comprising a composite layer, a core layer and a heat-sealing layer stacked in sequence, characterized in that: The composite layer is made of the following components in parts by weight: 30-40 parts of maleic anhydride grafted polypropylene, 40-50 parts of random copolymerized polypropylene, 5-10 parts of EVA, 10-20 parts of modified silicon dioxide and 5-8 parts of acrylate.
2. The anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to claim 1, characterized in that: The core layer is made of the following components in parts by weight: 45-65 parts of block copolymer polypropylene, 10-30 parts of POE, and 15-30 parts of ternary copolymer polypropylene; the heat sealing layer is made of the following components in parts by weight: 50-70 parts of binary copolymer polypropylene, 10-20 parts of POE, and 5-20 parts of homopolymer polypropylene.
3. The anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to claim 2, characterized in that: The weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C.
4. The anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to claim 1, characterized in that: The total thickness of the CPP film is 20-100 μm; the thickness of the composite layer is 10%-30% of the total thickness of the CPP film; and the thickness of the heat-sealing layer is 10%-30% of the total thickness of the CPP film.
5. The anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to claim 1, characterized in that: The preparation method of the modified silicon dioxide comprises the following steps: (1) dispersing silica into an ethanol / water mixture, then adding KH570, stirring for reaction, filtering, washing, and drying the product to obtain olefinated silica; (2) dispersing olefinated silica in tetrahydrofuran, then adding methacryloyloxyethyl trimethylammonium chloride, allyl acrylate, and oleyl palmitamide, ultrasonically treating, slowly adding dibenzoyl peroxide under stirring, polymerizing under a nitrogen atmosphere, precipitating the product with anhydrous ether, washing with alcohol, and drying to obtain the modified silica.
6. The anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to claim 5, characterized in that: In step (1), the ethanol / water mixture is obtained by mixing anhydrous ethanol and deionized water in a volume ratio of 10:4-8, and the amount ratio of silicon dioxide, ethanol / water mixture and KH570 is 10g:100mL:1-5g.
7. The anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to claim 5, characterized in that: In step (1), the stirring reaction condition is 50-65° C. for 1-4 h.
8. The anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to claim 5, characterized in that: In step (2), the ultrasonic treatment time is 20 to 40 minutes, and the polymerization reaction conditions are polymerization at 50 to 65° C. for 18 to 36 hours.
9. The anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to claim 5, characterized in that: In step (2), the mass ratio of olefinated silica, methacryloyloxyethyl trimethylammonium chloride, allyl acrylate, and oleyl palmitamide is 10:2-12:0.5-3:2-12; and the amount of dibenzoyl peroxide used is 0.1% to 1% of the total mass of the monomers.
10. A method for preparing an anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: the raw materials are melted respectively through three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
Citation Information
Patent Citations
CPP (Chlorinated Polypropylene) for aluminum plastic film and production method of CPP
CN112918054A