Method for reducing magnetic leakage of rotor of embedded permanent magnet motor and rotor magnetic isolation bridge nitriding method

By nitriding the magnetic isolation bridge part of the inner permanent magnet motor rotor core, the problem of the inability to reduce the width of the magnetic isolation bridge is solved, the magnetic leakage is reduced, efficiency and reliability are improved, and the motor performance is improved .

CN119051367APending Publication Date: 2024-11-29QINGDAO HAILIAN JINHUI MOTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410972076.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The width of the existing embedded permanent magnet motor rotor isolation bridge cannot be further reduced to reduce magnetic leakage, affecting the efficiency and reliability of the motor.

Method used

By nitriding the magnetic isolation bridge part of the rotor core, the material properties are changed, and the magnetic conductivity is reduced to reduce magnetic leakage.

Benefits of technology

It effectively reduces the magnetic leakage of the rotor, improves the back electromotive force and efficiency, reduces noise, and ensures the reliability of the motor rotor, without reducing the width of the magnetic isolation bridge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119051367A_ABST
    Figure CN119051367A_ABST
Patent Text Reader

Abstract

The invention discloses a method for reducing magnetic leakage of an embedded permanent magnet motor rotor and a rotor magnetic isolation bridge nitriding method, and belongs to the technical field of motors. The invention discloses a method for reducing magnetic leakage of an embedded permanent magnet motor rotor. Nitriding treatment is carried out on a magnetic isolation bridge part of a rotor iron core. By nitriding the magnetic isolation bridge part of the rotor iron core, the property of the magnetic isolation bridge material is changed, the magnetic leakage of the rotor can be reduced, the back electromotive force can be improved, the efficiency of the motor can be improved, the noise of the motor can be reduced, and the reliability of the motor rotor is ensured. The rotor iron core is installed in the motor rotor magnetic isolation bridge nitriding tool, then the tool is placed in an ion glow nitriding furnace for nitriding treatment, and by means of the grooves formed in the tool, only the magnetic isolation bridge part of the rotor iron core can be nitrided, the magnetic permeability of the magnetic isolation bridge part is reduced, and the magnetic permeability of other parts of the rotor iron core is not changed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for reducing magnetic leakage of an embedded permanent magnet motor rotor, belonging to the technical field of motors. The invention also relates to a method for nitriding a magnetic isolation bridge of a motor rotor. Background Art

[0002] The rotor core of the embedded permanent magnet motor mainly includes the rotor shaft hole, rotor magnetic steel slots, rotor magnetic isolation bridge, rotor outer circle, etc. Among them, the rotor magnetic bridge is the core part and the main part affecting the efficiency and reliability of the motor. The rotor core of the existing embedded permanent magnet motor mostly adopts a magnetic isolation bridge. Reducing the width of the magnetic isolation bridge can reduce leakage magnetism, increase back electromotive force, improve efficiency, and reduce noise, but its width cannot be too small. If the width of the magnetic isolation bridge is less than the thickness of the lamination, it will affect the mechanical strength of the punching sheet, fail to meet the process requirements, and cannot be mass-produced, while affecting the reliability of the motor rotor.

[0003] How to reduce magnetic leakage without reducing the width of the magnetic isolation bridge is an urgent problem that technicians need to solve. Summary of the invention

[0004] In view of the above-mentioned defects existing in the prior art, the present invention provides a method for reducing the magnetic leakage of the rotor of an embedded permanent magnet motor.

[0005] The present invention is realized by the following technical scheme: a method for reducing magnetic leakage of an embedded permanent magnet motor rotor, characterized in that the magnetic isolation bridge portion of the rotor core is subjected to nitriding treatment.

[0006] In the present invention, by nitriding the magnetic isolation bridge portion of the rotor core, the material properties of the magnetic isolation bridge are changed, and its magnetic permeability is reduced, which can reduce rotor leakage, increase back electromotive force, improve efficiency, and reduce noise.

[0007] Furthermore, the thickness of the nitriding layer at the magnetic isolation bridge of the rotor core is 0.5-0.7 mm.

[0008] The present invention also provides a method for nitriding a magnetic isolation bridge of a motor rotor, and the technical solution adopted is: a method for nitriding a magnetic isolation bridge of a motor rotor, characterized in that: it includes a motor rotor magnetic isolation bridge nitriding tool, the motor rotor magnetic isolation bridge nitriding tool includes a tool base, an end plate, and an end plate fixing structure, the tool base is a cylindrical structure with an open top and a bottom plate at the bottom, the cylindrical structure has a storage space for accommodating a coaxially arranged rotor core, a plurality of grooves that penetrate the height of the cylindrical wall are evenly opened on the cylindrical wall of the cylindrical structure, the grooves divide the cylindrical wall of the cylindrical structure into a plurality of guard teeth, the number of the grooves and the guard teeth is the same as the number of rotor poles, and the spacing between the grooves and the rotor core is The magnetic bridge parts correspond to each other, and the end plate is a disc that can match the inner diameter of the open end of the tooling base; the rotor core is installed into the tooling base of the motor rotor magnetic isolation bridge nitriding tooling, and the groove of the tooling base is aligned with the magnetic isolation bridge part of the rotor core, the end plate is placed on the upper part of the rotor core and fixedly connected to the tooling base through the end plate fixing structure; the tooling with the rotor core is placed on the cathode disk in the ion glow nitriding furnace, and the equipment is started to perform glow ion nitriding treatment on the workpiece on the cathode disk. The positive ions formed by the glow discharge bombard the magnetic isolation bridge part of the rotor core through the groove of the tooling base under the action of the high voltage electric field, so that a nitriding layer is formed on the magnetic isolation bridge part of the rotor core.

[0009] In the present invention, by placing the rotor core into the motor rotor magnetic isolation bridge nitriding tooling, and then placing the tooling with the rotor core into the ion glow nitriding furnace for nitriding treatment, the magnetic isolation bridge part of the rotor core is nitrided because it is not protected by the guard teeth and end plates, while the other parts of the rotor core are protected by the guard teeth, end plates, etc. of the tooling and their magnetic permeability remains unchanged. After the nitriding treatment, the magnetic resistance of the magnetic bridge increases, which can effectively reduce the rotor leakage.

[0010] Furthermore, during glow ion nitriding, the ion glow nitriding furnace is first evacuated, and when the pressure in the furnace drops to about 6Pa, ammonia is then filled in, and the pressure in the furnace is maintained at 1.3×100~1.3×1000Pa.

[0011] Furthermore, the temperature during glow ion nitriding is 1000-1100°C.

[0012] Furthermore, the thickness of the nitriding layer is 0.5-0.7 mm.

[0013] Furthermore, the inner diameter of the cylindrical structure of the tooling base is 0.02 mm-0.05 mm larger than the outer diameter of the rotor core.

[0014] Furthermore, a circular hole is provided at the center of the bottom plate of the tooling base, a threaded hole is provided at the center of the end plate, and the tooling base, the rotor core, and the end plate are fixedly connected together by screws passing through the centers thereof. The end plate, the rotor core, and the tooling base can be conveniently fixed together by screws.

[0015] Furthermore, the outer circumference of the end plate is provided with a plurality of end plate mounting protrusions protruding outward, the end plate mounting protrusions correspond to the tooth guards of the tooling base, the inner side of the tooth guard of the tooling base is provided with an end plate mounting groove at the position where it cooperates with the end plate, and the end plate is connected with the end plate mounting groove on the inner side of the tooth guard of the tooling base through its end plate mounting protrusions.

[0016] The beneficial effects of the present invention are as follows: the present invention changes the material properties of the magnetic isolation bridge by subjecting the magnetic isolation bridge of the rotor core to nitriding treatment, which can reduce the magnetic leakage of the rotor, increase the back electromotive force by 1.5-3%, improve the motor efficiency by 0.5-1.5%, and reduce the noise of the motor. At the same time, since the magnetic leakage of the rotor can be reduced by only subjecting the magnetic isolation bridge of the rotor core to nitriding treatment, it is not necessary to reduce the magnetic leakage by reducing the width of the magnetic isolation bridge, thus ensuring the reliability of the motor rotor. The nitriding tooling structure of the magnetic isolation bridge of the motor rotor in the present invention is reasonably designed. After the rotor core is installed in the tooling and the end plate is installed, only the magnetic isolation bridge of the rotor core is exposed from the groove on the tooling base, and the rest of the rotor core is protected by the guard teeth, the end plate and the bottom plate. When the rotor core installed in the tooling is placed in a nitriding furnace for nitriding treatment, the magnetic isolation bridge is not protected by the guard teeth and the end plate, so it is nitrided. The method of the present invention can reliably perform nitriding treatment on the magnetic isolation bridge part of the rotor core to reduce its magnetic permeability, and can reliably protect other parts of the rotor core to ensure that the magnetic permeability of other parts remains unchanged. The method is simple and reliable. In addition, the present invention adopts ion nitriding method and directly heats the workpiece by glow discharge. No special heating and heat preservation equipment is required to obtain uniform temperature distribution. Compared with the indirect heating method, the heating efficiency can be increased by more than 2 times to achieve energy saving effect. According to actual measurement, its energy consumption is only 40-70% of gas nitriding. The tooling used in the present invention has a simple structure and is easy to operate. The installation and removal of the rotor core in the tooling are simple and convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the structure of the present invention in Example 1;

[0018] Figure 2 is a cross-sectional schematic diagram of the present invention in Example 1;

[0019] Figure 3 is a schematic diagram of the three-dimensional structure of the present invention in Example 1;

[0020] Figure 4is a schematic front view of the tooling base in Example 1;

[0021] Figure 5 yes Figure 4 Schematic diagram of top view;

[0022] Figure 6 is a cross-sectional schematic diagram of the tooling base in Example 1;

[0023] Figure 7 is a schematic diagram of the three-dimensional structure of the tooling base in Example 1;

[0024] Figure 8 It is a schematic diagram of the end face of the rotor core;

[0025] Fig. 9 is a schematic side view of the rotor core;

[0026] Fig.10 It is a schematic end view of the cooperation between the rotor core and the tooling base in Example 1;

[0027] Fig.11 is a front view schematic diagram of the end plate in Example 2;

[0028] Fig.12 yes Fig.11 Schematic diagram of top view;

[0029] Fig.13 is a schematic diagram of the three-dimensional structure of the end plate in Example 2;

[0030] Fig.14 is a schematic front view of the tooling base in Example 2;

[0031] Fig.15 yes Fig.14 Schematic diagram of top view;

[0032] Fig.16 is a schematic cross-sectional view of the tooling base in Example 2;

[0033] Fig.17 is a schematic diagram of the three-dimensional structure of the tooling base in Example 2;

[0034] Fig.18 is a schematic diagram of the coordination between the rotor core and the tooling in Example 2;

[0035] In the figure, 1, tooling base, 2, rotor core, 3, end plate, 4, screws;

[0036] 1.1, circular hole in the center of the bottom plate, 1.2, tooth guard, 1.3, groove, 1.4, bottom plate, 1.5, end plate mounting groove;

[0037] 2.1, magnetic isolation bridge, 2.2, shaft hole, 2.3, magnetic steel slot, 2.4, outer circle of iron core;

[0038] 3.1. End plate installation boss. DETAILED DESCRIPTION

[0039] The present invention will be further described below by way of non-limiting embodiments and in conjunction with the accompanying drawings:

[0040] A method for reducing magnetic leakage of an embedded permanent magnet motor rotor, the technical solution of which is: nitriding the magnetic isolation bridge of the rotor core. Preferably, the thickness of the nitriding layer of the magnetic isolation bridge of the rotor core is 0.5-0.7 mm.

[0041] The present invention also provides a method for nitriding a magnetic isolation bridge of a motor rotor, as follows:

[0042] Example 1

[0043] The invention discloses a motor rotor magnetic separation bridge nitriding method, comprising a motor rotor magnetic separation bridge nitriding tool and an ion glow nitriding furnace. The motor rotor magnetic separation bridge nitriding tool is used to install the rotor core so as to place the rotor core in the ion glow nitriding furnace for nitriding treatment. The ion glow nitriding furnace is a prior art.

[0044] As attached Figure 1-Figure 7 As shown, the motor rotor magnetic isolation bridge nitriding tooling includes a tooling base 1, an end plate 3, and an end plate fixing structure. The tooling base 1 is a cylindrical structure with an open top and a bottom plate 1.4 at the bottom. A circular hole 1.1 is arranged at the center of the bottom plate 1.4. The cylindrical structure has a storage space for accommodating a coaxially arranged rotor core. A plurality of grooves 1.3 that penetrate the height of the cylindrical wall are evenly opened on the cylindrical wall of the cylindrical structure. The grooves 1.3 divide the cylindrical wall of the cylindrical structure into a plurality of guard teeth 1.2. The number of the grooves 1.3 and the guard teeth 1.3 is the same as the number of rotor poles, and the grooves 1.3 correspond to the magnetic isolation bridge position of the rotor core. The end plate 3 is a disc that can match the inner diameter of the open end of the tooling base 1, and a threaded hole is arranged at the center of the end plate 3. The end plate fixing structure includes a screw 4, which can pass through the circular hole 1.1 at the center of the bottom plate of the tooling base 1 and connect with the threaded hole at the center of the end plate 3.

[0045] In order to facilitate the removal of the rotor core from the tooling base 1, a clearance fit is adopted between the rotor core and the tooling base. Preferably, the inner diameter of the cylindrical structure is 0.02mm-0.05mm larger than the outer diameter of the rotor core.

[0046] In this embodiment, the tooling base 1 is provided with 6 grooves 1.3 and 6 tooth guards 1.2, and the grooves 1.3 and the tooth guards 1.2 are evenly spaced.

[0047] As attached Figure 8-Figure 9The figure shows a schematic diagram of a rotor core of an embedded permanent magnet motor. The structure of the rotor core 2 is the prior art, which includes a magnetic isolation bridge 2.1, an axial hole 2.2, a magnetic steel slot 2.3, an outer circle of the core 2.4, etc.

[0048] As attached Fig.10 As shown, before nitriding treatment, the rotor core 2 is installed into the tooling base 1 of the motor rotor magnetic isolation bridge nitriding tooling, and the grooves 1.3 of the tooling base 1 are respectively aligned with the magnetic isolation bridge parts of the corresponding positions of the rotor core 2, and then the end plate 3 is placed on the upper part of the rotor core 2, and the screw 4 is passed through the circular hole 1.1 in the center of the bottom plate 1.4 and the axial hole 2.2 of the rotor and then threadedly connected with the threaded hole in the center of the end plate 3, so that the rotor core 2 is fixed in the tooling base 1.

[0049] During ion nitriding, the tooling with the rotor core 2 is placed on the cathode disk in the ion glow nitriding furnace, and the power supply is connected to evacuate. When the pressure in the furnace drops to about 6Pa, ammonia is filled in, and the pressure in the furnace is maintained in the range of 1.3×100~1.3×1000Pa. High-voltage direct current is applied between the cathode (workpiece) and the anode (furnace body) to perform glow ion nitriding on the workpiece. Due to the low pressure in the furnace and the subsequent glow discharge heating, the ammonia entering the furnace will decompose. The gas volume fraction obtained by the reaction in the furnace is a low-pressure environment of 25% N2 and 75% H2. The temperature during glow ion nitriding is 1000-1100℃.

[0050] The principle of glow ion nitriding is: when high voltage direct current is applied between the cathode (workpiece) and the anode (furnace body), glow discharge occurs in the furnace. At this time, the low-pressure gas in the furnace is ionized under the action of the high voltage electric field, and ionized into positively charged N and H ions and negatively charged electrons. The positive ions formed by the glow discharge move in a directional manner under the action of the high voltage electric field, that is, bombarding the cathode (workpiece) surface at a very high speed, and a series of physical and chemical phenomena occur on the surface of the workpiece to form a nitriding layer.

[0051] In the present invention, when the fixture equipped with the rotor core 2 is subjected to nitriding treatment on the cathode disk in the ion glow nitriding furnace, the positive ions formed by the glow discharge bombard the surface of the magnetic isolation bridge of the rotor core at a very high speed through the groove 1.3 of the fixture base 1 under the action of the high voltage electric field, so that a nitriding layer is formed on the surface of the magnetic isolation bridge of the rotor core. The other parts of the rotor core are protected by the teeth, end plates, etc. of the fixture, and their magnetic permeability remains unchanged.

[0052] The other parts of this embodiment are all prior art and will not be described in detail here.

[0053] Example 2

[0054] As attached Figure 11-Figure 18As shown, this embodiment is basically the same as Embodiment 1, except that the end plate fixing structure adopted by the tooling in this embodiment is different from that in Embodiment 1.

[0055] In this embodiment, no circular hole is provided at the center of the bottom plate 1.4 of the tooling base 1, and no threaded hole is provided at the center of the end plate 3 either.

[0056] In this embodiment, the outer circumference of the end plate 3 is provided with a plurality of end plate mounting protrusions 3.1 protruding outward, the end plate mounting protrusions 3.1 correspond to the tooth guards 1.2 of the tool base 1, and the inner side of the tooth guards 1.2 of the tool base 1 is provided with end plate mounting grooves 1.5 at the position where the tooth guards 1.2 of the tool base 1 cooperate with the end plate 3. The end plate 3 is connected with the end plate mounting grooves 1.5 on the inner side of the tooth guards 1.2 of the tool base 1 through its end plate mounting protrusions 3.1.

[0057] When installing the rotor core 2, the rotor core 2 is installed into the tooling base 1, and each groove 1.3 is aligned with the magnetic isolation bridge part at the corresponding position of the rotor core 2, and then the end plate 3 is placed on the upper part of the rotor core 2, and the end plate mounting protrusion 3.1 of the end plate 3 is inserted or screwed into the end plate mounting groove 1.5 on the inner side of the guard tooth 1.2, so as to fix the rotor core 2 in the tooling base 1.

[0058] The other parts of this embodiment are the same as those of Embodiment 1 and will not be described again.

Claims

1. A method for reducing magnetic flux leakage of an embedded permanent magnet motor rotor. Its characteristics are: The magnetic isolation bridge area of ​​the rotor core is nitrided.

2. The method for reducing magnetic flux leakage of an embedded permanent magnet motor rotor according to claim 1, Its characteristics are: The thickness of the nitriding layer at the magnetic isolation bridge of the rotor core is 0.5-0.7mm.

3. A method for nitriding a motor rotor magnetic bridge, Its characteristics are: The invention comprises a motor rotor magnetic isolation bridge nitriding tool, the motor rotor magnetic isolation bridge nitriding tool comprises a tool base (1), an end plate (3), and an end plate fixing structure. The tool base (1) is a cylindrical structure with an open top and a bottom plate at the bottom. The cylindrical structure has a storage space for accommodating a coaxially arranged rotor core. A plurality of grooves (1.3) penetrating the height of the cylindrical wall are evenly opened on the cylindrical wall of the cylindrical structure. The grooves (1.3) separate the cylindrical wall of the cylindrical structure into a plurality of guard teeth (1.2). The number of the grooves (1.3) and the guard teeth (1.3) is the same as the number of rotor poles, and the grooves (1.3) correspond to the magnetic isolation bridge portion of the rotor core. The end plate (3) is a structure that can be connected with the cylindrical wall. The tool base (1) is provided with a disc having a matching inner diameter at the open end thereof; the rotor core is installed into the tool base (1) of the motor rotor magnetic isolation bridge nitriding tool, and the groove (1.3) of the tool base (1) is aligned with the magnetic isolation bridge portion of the rotor core, and the end plate (3) is placed on the upper part of the rotor core and fixedly connected to the tool base (1) through the end plate fixing structure; the tool with the rotor core installed is placed on the cathode disk in the ion glow nitriding furnace, and the equipment is started to perform glow ion nitriding treatment on the workpiece on the cathode disk, and the positive ions formed by the glow discharge bombard the magnetic isolation bridge portion of the rotor core through the groove (1.3) of the tool base (1) under the action of the high voltage electric field, so that a nitriding layer is formed on the magnetic isolation bridge portion of the rotor core.

4. The motor rotor magnetic bridge nitriding method according to claim 3, Its characteristics are: During glow ion nitriding, the ion glow nitriding furnace is first evacuated. When the pressure in the furnace drops to about 6Pa, ammonia is filled in and the pressure in the furnace is maintained at 1.3×100~1.3×1000Pa.

5. The motor rotor magnetic bridge nitriding method according to claim 4, Its characteristics are: The temperature during glow ion nitriding is 1000-1100℃.

6. The motor rotor magnetic bridge nitriding method according to claim 3, 4 or 5, Its characteristics are: The thickness of the nitriding layer is 0.5-0.7mm.

7. The motor rotor magnetic bridge nitriding method according to claim 3, 4 or 5, Its characteristics are: The inner diameter of the cylindrical structure of the tooling base (1) is 0.02 mm to 0.05 mm larger than the outer diameter of the rotor core.

8. The motor rotor magnetic bridge nitriding method according to claim 7, Its characteristics are: A circular hole is provided at the center of the bottom plate of the tooling base (1), and a threaded hole is provided at the center of the end plate (3); the tooling base (1), the rotor core, and the end plate (3) are fixedly connected together by screws (4) passing through the centers thereof.

9. The motor rotor magnetic bridge nitriding method according to claim 7, Its characteristics are: The outer circumference of the end plate (3) is provided with a plurality of end plate mounting protrusions (3.1) protruding outward, the end plate mounting protrusions (3.1) corresponding to the tooth guards (1.2) of the tooling base (1), the inner side of the tooth guards (1.2) of the tooling base (1) is provided with an end plate mounting groove (1.5) at the position where the tooth guards (1.2) of the tooling base (1) cooperate with the end plate (3), and the end plate (3) is connected to the end plate mounting groove (1.5) on the inner side of the tooth guards (1.2) of the tooling base (1) through its end plate mounting protrusions (3.1).