Photoetching method of phase change material layer

By using silicon-containing antireflection layer and wet removal of photoresist layer in GST layer lithography, the problems of SiO2 layer unevenness and ashing process produce particulate matter, achieving higher consistency and yield, avoiding The electrical properties are affected and the photolithography accuracy and product quality are improved.

CN119053236APending Publication Date: 2024-11-29BEIJING ADVANCED MEMORY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411037850.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the photolithography method of the GST layer is defective due to the inhomogeneity of the SiO2 layer and the product falling on the GST layer during the etching process. The ashing process during photolithography is used to affect electrical properties, reducing product yield. .

Method used

The photoresist layer is removed by wet method by using the laminated body including a phase change material layer, a titanium nitride layer, a first carbon mask layer, a first silicon-containing antireflection layer, and a first photoresist layer formed in sequence from bottom to top. The silicon-containing antireflection layer is etched, and a new carbon mask and antireflection layer are formed in the photolithography rework step. The ashing process is used to remove the carbon mask layer to avoid the generation of particulate matter.

Benefits of technology

It improves the photolithography consistency and product yield of the GST layer, avoids the influence of electrical properties, and enhances the photolithography accuracy and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053236A_ABST
    Figure CN119053236A_ABST
Patent Text Reader

Abstract

The invention provides a photoetching method of a GST layer, and belongs to the field of semiconductor integrated circuit manufacturing. The method according to the present invention comprises: a laminate forming step; a photoetching step; a wet photoresist removal step: if the process requirement is not met, spraying a solvent to the first patterned photoresist layer so as to remove the first patterned photoresist layer; a silicon-containing anti-reflection layer removing step of etching the first silicon-containing anti-reflection layer so as to remove the first silicon-containing anti-reflection layer; a first carbon mask layer removal step: removing the first carbon mask layer by adopting an ashing process; and a photoetching reworking step: sequentially forming a second carbon mask layer, a second silicon-containing anti-reflection layer and a second photoresist layer on the silicon nitride layer, and then exposing and developing the second photoresist layer to form a second patterned photoresist layer. According to the method provided by the invention, the electrical property of the product is not influenced, and the product yield can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor integrated circuit manufacturing, and in particular to a photolithography method for a phase change material layer. Background Art

[0002] In the manufacture of semiconductor integrated circuits, especially in the manufacture of phase change memory, the requirements for the photolithography of the GST (phase change material) layer are getting higher and higher. Figure 4 As shown, in the prior art, the etching of the GST layer 91 usually forms a TiN (titanium nitride) layer 92, a SiN (silicon nitride) layer 93, a carbon HM (mask) layer 94, a SiO2 (silicon dioxide) layer 97, an ARC layer (anti-reflective layer) 95, and a PR (photoresist) layer 96 on the GST layer 91 in sequence, thereby forming a laminate 900. Then, the PR layer 96 is photolithographically processed to form a patterned PR layer. Then, the ARC layer 95, the SiO2 layer 97, the carbon HM layer 94, the SiN layer 93, the TiN layer 92, and the GST layer 91 are etched in sequence through the patterned PR layer to form a patterned GST layer.

[0003] Among them, the function of the ARC layer 95 is to absorb reflected light in the photolithography process and improve the photolithography accuracy. The function of the SiO2 layer 97 is to serve as a mask in the etching process of the carbon HM layer 94. Because the PR layer 96 and the ARC layer 95 are relatively soft and cannot be used as a mask in the etching process of the carbon HM layer 94, a SiO2 layer 97 must be formed under the ARC layer 95, and the carbon HM layer 94 is etched using the SiO2 layer 97 as a mask. The SiO2 layer 97 is usually formed by a CVD (chemical vapor deposition) process, but the U% (thickness uniformity) of the SiO2 layer 97 formed in this way is not good, which will affect the CD (feature size) uniformity (Uniformity) of the PR layer 96 and the ARC layer 95 during photolithography, thereby affecting the CD uniformity of the final GST layer. In addition, some products will be generated when etching the SiO2 layer 97, and these products will eventually fall on the GST layer, causing defects.

[0004] In order to solve this problem, PCT / CN2023 / 123136 discloses a new laminate 800, such as Figure 5As shown, the laminate 800 includes a GST layer 801, a TiN layer 802, a SiN layer 803, a carbon HM layer 804, an SHB layer (Sirich hard mask bottom ARC, silicon-containing anti-reflection layer) 805, and a PR layer 806, which are formed in sequence from bottom to top. That is, the original ARC layer 95 and the SiO2 layer 97 are replaced by the SHB layer 805. The SHB layer 805 can play an anti-reflective role, and it contains silicon and has a relatively high hardness, so it can be used as a mask for etching the carbon HM layer 804. In this way, there is no need to form a SiO2 layer on the carbon HM layer 804. In addition, the U% of the SHB layer 805 is better, so the CD consistency of the final GST layer will be improved. In addition, because there is no SiO2 layer, the product generated when etching the SiO2 layer will not appear, and it will not fall on the GST layer to cause defects. This also reduces the defects on the final GST layer.

[0005] However, such a laminate 800 also has problems. For example, in the subsequent photolithography process, the PR layer 806 needs to be photolithographically processed to form a patterned PR layer 816. Figure 6 As shown. Then the patterned PR layer 816 is tested to confirm whether the patterned PR layer 816 meets the process requirements. If it does not meet the process requirements, photolithography rework is required, that is, the patterned PR layer 816 is removed, and then a layer of PR is re-applied and photolithography is performed again.

[0006] The prior art photolithography rework method is as follows Figure 7 As shown, the first step is to remove the patterned PR layer S801, and the patterned PR layer 816 is usually removed by an ashing process. The ashing process uses oxygen plasma to react with the high molecular weight compounds in the PR to generate volatile reactants, and finally remove the PR. In the original technology, the SiO2 layer 97 is below the PR layer 96 of the laminate 900, and there will be no problem in using the ashing process. However, for the laminate 800, the SHB layer 805 is below the PR layer 806. Due to the characteristics of the SHB layer 805 itself, some particles 817 will be generated after the ashing process. As shown in FIG. Figure 7 As shown, these particles 817 will adhere to the SHB layer 805, which will affect the subsequent steps.

[0007] In the subsequent SHB layer removal step S802, the SHB layer 805 is usually removed by etching. However, the particles 817 attached to the SHB layer 805 will prevent the SHB layer 805 below from being etched, thereby forming SHB residues 815. Fig. 9 shown.

[0008] In the subsequent carbon HM layer removal step S803, an ashing process is usually used to remove the carbon HM layer 4. After the carbon HM layer 4 is removed, the particles 817 and the SHB residues 815 will fall onto the SiN layer 803, and after the subsequent photolithography rework step S804, the particles 817 and the SHB residues 815 will still remain on the wafer, which will affect the electrical properties of the product and reduce the yield of the product.

[0009] Therefore, the industry is in urgent need of a GST layer photolithography method that will not affect the electrical properties of the product and can improve the product yield. Summary of the invention

[0010] The present invention aims to provide a GST layer photolithography method which will not affect the electrical properties of the product and can improve the product yield.

[0011] The photolithography method of the GST layer of the present invention comprises:

[0012] A laminate forming step, forming a laminate on a semiconductor substrate, wherein the laminate includes a phase change material layer, a titanium nitride layer, a silicon nitride layer, a first carbon mask layer, a first silicon-containing anti-reflection layer, and a first photoresist layer formed in sequence from bottom to top;

[0013] a photolithography step of exposing and developing the first photoresist layer to form a first patterned photoresist layer, and testing the first patterned photoresist layer to confirm whether the first patterned photoresist layer meets the process requirements;

[0014] a wet photoresist removal step, if the process requirement is not met, spraying a solvent onto the first patterned photoresist layer, thereby removing the first patterned photoresist layer;

[0015] a silicon-containing anti-reflection layer removal step, etching the first silicon-containing anti-reflection layer to remove the first silicon-containing anti-reflection layer;

[0016] a first carbon mask layer removal step, using an ashing process to remove the first carbon mask layer; and

[0017] The photolithography rework step sequentially forms a second carbon mask layer, a second silicon-containing anti-reflection layer, and a second photoresist layer on the silicon nitride layer, and then exposes and develops the second photoresist layer to form a second patterned photoresist layer.

[0018] The photolithography method of the GST layer of the present invention will not affect the electrical properties of the product and can improve the product yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a flow chart of a photolithography method for a GST layer of the present invention;

[0020] Figures 2 to 3 It is a schematic diagram of various steps of the photolithography method of the GST layer of the present invention;

[0021] Figures 4 to 6 is a schematic diagram of a prior art photolithography method;

[0022] Figure 7 is a flow chart of a prior art lithography method; and

[0023] Figure 8 and Fig. 9 It is a schematic diagram of various steps of the prior art photolithography method.

[0024] Explanation of symbols

[0025] 100, 800, 900 laminates

[0026] 1, 801, 901GST layer

[0027] 2, 802, 902TiN layer

[0028] 3, 803, 903SiN layer

[0029] 4First carbon HM layer

[0030] 5First SHB layer

[0031] 6First PR layer

[0032] 16 First patterned PR layer

[0033] 804, 904 carbon HM layer

[0034] 805, 905 SHB layer

[0035] 806, 906PR layer

[0036] 815SHB residue

[0037] 816 patterned PR layer

[0038] 817 particles DETAILED DESCRIPTION

[0039] Refer to the following Figures 1 to 3 The photolithography method of the GST layer of the present invention is described. Figure 1 As shown, the photolithography method of the GST layer of the present invention includes: a laminate forming step S001, a photolithography step S002, a wet first patterned PR layer removal step S003, a first SHB layer removal step S004, a first carbon HM layer removal step S005, and a photolithography rework step S006. Each step will be described in detail below with reference to the accompanying drawings.

[0040] The layered body forming step S001, Figure 2 As shown, a laminate 100 is formed on a semiconductor substrate (not shown), and the laminate 100 includes a GST layer 1, a TiN layer 2, a SiN layer 3, a first carbon HM layer 4, a first SHB layer 5, and a first PR layer 6 formed in sequence from bottom to top.

[0041] In this embodiment, a GST layer 1 and a TiN layer 2 are first formed on a semiconductor substrate by a PVD (physical vapor deposition) process. The GST layer 1 and the TiN layer 2 may be formed directly on the semiconductor substrate, or there may be other layers between the semiconductor substrate and the GST layer 1 and the TiN layer 2. Then a SiN layer 3 is formed on the TiN layer 2 by a CVD process. The SiN layer 3 may be formed directly on the TiN layer 2, or there may be other layers between the TiN layer 2 and the SiN layer 3. In addition, the SiN layer 3 may also be replaced by a SiO2 layer. Then a first carbon HM layer 4, a first SHB layer 5, and a first PR layer 6 are sequentially formed on the SiN layer 3 by a coating process.

[0042] Due to the properties of the GST layer 1 and the TiN layer 2, SiN needs to be used as a mask for etching. Therefore, it is necessary to first form a SiN layer 3 on the GST layer 1 and the TiN layer 2. Before etching the GST layer 1 and the TiN layer 2, the SiN layer 3 must be etched first to form a patterned SiN layer, and then the GST layer 1 and the TiN layer 2 are etched through the patterned SiN layer. Because the SiN layer 3 is relatively hard and difficult to etch, when etching the SiN layer 3, the first PR layer 6 and the first SHB layer 5 cannot be directly used as masks for the SiN layer 3. The first carbon HM layer 4 must be formed on the SiN layer 3, and the first carbon HM layer 4 must be used as a mask for etching the SiN layer 3.

[0043] Photolithography step S002, such as Figure 3 As shown, the first PR layer 6 is exposed and developed to form a first patterned PR layer 16. The first PR layer 6 can be exposed and developed in any suitable manner in the prior art, which will not be described in detail herein. The first patterned PR layer 16 is then tested to confirm whether the first patterned PR layer 16 meets the process requirements.

[0044] In this embodiment, it is to detect whether the CD of the first patterned PR layer 16 is too large or too small, and whether the number of large particles is too large. In other embodiments, other detections may also be performed.

[0045] In the wet first patterned PR layer removal step S003, if the process requirements are not met, a solvent is sprayed onto the first patterned PR layer 16, thereby removing the first patterned PR layer 16. In this embodiment, an organic solvent is sprayed onto the first patterned PR layer 16 by a nozzle of a PR removal machine, and the wafer is rotated rapidly at the same time, so that the organic solvent reacts fully with the PR, thereby cleaning off the first patterned PR layer 16. In this embodiment, the organic solvent is EBR 7030, and the PR removal machine is TELLITHOUS PRO I of TEL Corporation of Japan. In other embodiments, other suitable organic solvents and other suitable machines may also be used.

[0046] Through the wet first patterned PR layer removal step S003, the first patterned PR layer 16 can be fully removed, and the experimental results show that the first patterned PR layer 16 is removed by this method without generating particles as in the case of an ashing process, which will not affect the subsequent steps.

[0047] However, the use of solvent cleaning to remove the first patterned PR layer 16 will cause a certain degree of damage to the underlying first SHB layer 5, thereby making the upper surface of the first SHB layer 5 uneven. The damaged first SHB layer 5 cannot be used anymore, otherwise it will also affect the subsequent steps. Therefore, the first SHB layer 5 must also be removed and a new SHB layer must be coated.

[0048] In the first SHB layer removing step S004 , the first SHB layer 5 is etched to remove the first SHB layer 5 .

[0049] Because the first patterned PR layer 16 has been fully removed in the wet first patterned PR layer removal step S003 without generating any particles, when etching the first SHB layer 5, the first SHB layer 5 can also be fully etched away without generating any SHB residues as in the prior art, which will not affect the subsequent steps.

[0050] However, in the process of etching the first SHB layer 5, the first carbon HM layer 4 below will be damaged, so that the upper surface of the first carbon HM layer 4 becomes uneven. The damaged first carbon HM layer 4 cannot be used anymore, otherwise it will also affect the subsequent steps. Therefore, the first carbon HM layer 4 must also be removed and a new carbon HM layer must be coated.

[0051] In the first carbon HM layer removal step S005 , the first carbon HM layer 4 is removed by an ashing process.

[0052] Because in the wet first patterned PR layer removal step S003 and the first SHB layer removal step S004, the first patterned PR layer 16 and the first SHB layer 5 have been fully removed, and no particles and SHB residues are generated, so that the subsequent steps will not be affected. In addition, in the process of removing the first carbon HM layer 4 by the ashing process, the underlying SiN layer 3 will not be damaged, so there is no need to remove the SiN layer 3 and then re-form a new SiN layer.

[0053] In the photolithography rework step S006 , a second carbon HM layer, a second SHB layer, and a second PR layer are sequentially formed on the SiN layer 3 , and then the second PR layer is exposed and developed to form a second patterned PR layer.

[0054] The first SHB layer 5, the first carbon HM layer 4 and the photolithography rework may be removed by any suitable method in the prior art, which will not be described in detail herein.

[0055] The photolithography method of the GST layer of the present invention will not affect the electrical properties of the product and can improve the product yield.

[0056] Although the present invention has been disclosed in the above embodiments, it is not intended to limit the present invention. Any professional and technical personnel in the field may make various necessary changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined by the attached claims.

Claims

1. A photolithography method for a phase change material layer, comprising: A laminate forming step S001, forming a laminate (100) on a semiconductor substrate, wherein the laminate (100) comprises a phase change material layer (1), a titanium nitride layer (2), a silicon nitride layer (3), a first carbon mask layer (4), a first silicon-containing anti-reflection layer (5), and a first photoresist layer (6) formed in sequence from bottom to top; Photolithography step S002, exposing and developing the first photoresist layer (6) to form a first patterned photoresist layer (16), and testing the first patterned photoresist layer (16) to confirm whether the first patterned photoresist layer (16) meets the process requirements; Wet photoresist removal step S003: if the process requirement is not met, spraying a solvent onto the first patterned photoresist layer (16), thereby removing the first patterned photoresist layer (16); A silicon-containing anti-reflection layer removal step S004, etching the first silicon-containing anti-reflection layer (5), thereby removing the first silicon-containing anti-reflection layer (5); A first carbon mask layer removal step S005, using an ashing process to remove the first carbon mask layer (4); and In the photolithography rework step S006, a second carbon mask layer, a second silicon-containing anti-reflection layer, and a second photoresist layer are sequentially formed on the silicon nitride layer (3), and then the second photoresist layer is exposed and developed to form a second patterned photoresist layer.