Powdered binder for secondary battery positive electrode and use thereof

By using a non-crosslinked polymer with moderate glass transition temperature as powdered adhesive, the problems of low positive electrode productivity and poor adhesive dispersion of secondary batteries are solved, and more efficient electrode mixture layer formation and adhesion are achieved. .

CN119054112APending Publication Date: 2024-11-29TOAGOSEI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028910.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The powdered adhesive of the positive electrode of the conventional secondary battery has a high heating and welding temperature and insufficient adhesion between the adhesive and the active substance, resulting in low productivity and poor dispersion.

Method used

A non-crosslinked polymer containing a glass transition temperature of 60°C or above and 150°C or below is used as a powdered adhesive, and a specific structural unit and particle size range are combined to form a powdered particle composite to improve the dispersion of the adhesive. Sex and closeness.

Benefits of technology

The productivity of the positive electrode of the secondary battery and the dispersion and adhesion of the adhesive in the active substance are improved, thereby achieving a more efficient formation of the electrode mixture layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005051300880000181
    Figure BDA0005051300880000181
  • Figure BDA0005051300880000201
    Figure BDA0005051300880000201
Patent Text Reader

Abstract

Provided is a powdered binder for a secondary battery positive electrode, which is capable of improving the productivity of a secondary battery positive electrode, and is capable of improving the dispersibility of the binder in an active material and the adhesion to the active material. Also provided is a powdery particle composite containing the powdery binder. A powder binder for a secondary battery positive electrode, the powder binder for a secondary battery positive electrode containing a non-crosslinked polymer having a glass transition temperature of 60 DEG C to 150 DEG C (inclusive). Also disclosed is a powdered particle composite which contains a positive electrode active material and the powdered binder for the positive electrode of a secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This specification relates to a powdery binder for a secondary battery positive electrode and its use. Background Art

[0002] As a secondary battery, various power storage devices such as nickel-metal hydride secondary batteries, lithium-ion secondary batteries, and double-layer capacitors are put into practical use. These electrodes for secondary batteries are made by coating and drying the composition on the collector, wherein the composition is a composition for forming an electrode mixture layer containing an active material and an adhesive. For example, in a lithium-ion secondary battery, as an adhesive for a negative electrode mixture layer composition, an aqueous adhesive containing styrene butadiene rubber (SBR) latex and carboxymethyl cellulose (CMC) is used. On the other hand, as an adhesive for a positive electrode mixture layer, N-methyl-2-pyrrolidone (NMP) solution of polyvinylidene fluoride (PVDF) is widely used.

[0003] In recent years, as the use of various secondary batteries has expanded, there has been a growing demand for improved energy density, reliability, durability, and productivity of secondary batteries. Under such circumstances, electrodes for secondary batteries are also required to have both higher performance and productivity.

[0004] The electrode for secondary battery is an electrode in which an electrode mixture layer is laminated on a collector foil, wherein the electrode mixture layer is an electrode mixture layer formed by bonding an active material and a conductive auxiliary agent by a binder. In the manufacture of the electrode, a method of applying an electrode slurry on the collector and drying the electrode slurry is generally adopted, wherein the electrode slurry is an electrode slurry containing an active material, a conductive auxiliary agent, a binder (adhesive), etc. For example, in the manufacturing process of the positive electrode of a secondary battery, an electrode slurry containing a positive electrode active material, a conductive auxiliary agent, a binder, and an organic solvent is used.

[0005] However, when removing the organic solvent from the electrode slurry, a large amount of thermal energy is required (such as a prolonged drying time), and therefore it is difficult to improve productivity.

[0006] Therefore, as a method for producing a positive electrode for a secondary battery, a method (so-called “dry mixing”) using a mixed powder containing an active material (hereinafter simply referred to as “mixed powder”) instead of an electrode slurry has been proposed. As a mixed powder, for example, Patent Document 1 describes a mixed powder containing active material powder and binder (adhesive) powder, and the embodiment specifically discloses a mixed powder, wherein the mixed powder contains lithium manganate powder (positive electrode active material) as active material powder and PVDF powder as binder powder. It is shown that the mixed powder is attached to the collector by powder coating, and the mixed powder attached to the collector is heated to a softening temperature (150° C.) or above of the binder to be welded, thereby forming an electrode mixture layer (active material layer) with high film thickness accuracy and good load characteristics without using electrode slurry (active material paste).

[0007] In addition, Patent Document 2 describes a mixed powder (powdered composite particles) formed of a polymer having a glass transition temperature of 35°C to 80°C and a volume-based D50 average particle size of primary particles of 80nm to 1000nm, and a volatile component of less than 1% by weight at 120°C. The embodiment specifically discloses a mixed powder comprising NMC powder (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, positive electrode active material), "a cross-linked polymer having structural units derived from a non-cross-linking monomer (main component: ethyl methacrylate) and a cross-linking monomer (allyl methacrylate)" as a binder powder. It is shown that since no electrode slurry is used when forming the electrode mixture layer, the productivity of the electrode for secondary batteries is excellent, and since no water-soluble polymer component is required as a dispersant, low resistance can be achieved, and the thickness accuracy and flexibility of the resulting electrode can be formed. Prior art literature Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2001-351616 Patent Document 2: International Publication No. 2014 / 192652 Summary of the invention Technical problem to be solved by the invention

[0009] Although the powdered binder (PVDF) disclosed in Patent Document 1 can be used to manufacture electrodes for secondary batteries by dry mixing without using electrode slurry, after the mixed powder is attached to the surface of the collector, the heating and welding temperature needs to be above 150°C (200°C in the embodiment), so there are problems in productivity and there are deficiencies in the adhesion between the powdered binder and the active material.

[0010] On the other hand, the powdered binder (the above-mentioned cross-linked polymer) disclosed in Patent Document 2 can be press-formed (compressed) at a lower temperature than the above-mentioned PVDF after the mixed powder is attached to the surface of the collector, but the binders are easily welded together, and the binder has deficiencies in terms of dispersibility in the active material and adhesion with the active material.

[0011] The present invention is an invention completed in view of such a situation, and its purpose is to provide a powdery binder for a secondary battery positive electrode, the powdery binder for a secondary battery positive electrode can improve the productivity of the secondary battery positive electrode, and can improve the dispersibility of the binder in the active material and the adhesion with the active material. In addition, a powdery particle complex containing the above-mentioned powdery binder, a secondary battery positive electrode obtained using the powdery particle complex, and a secondary battery are provided. Technical means to solve technical problems

[0012] The present inventors conducted intensive research to solve the above-mentioned problems and found that by using a powdered binder for a secondary battery positive electrode containing a non-cross-linked polymer with a glass transition temperature in a specific range, the productivity of the secondary battery positive electrode can be improved, and the dispersibility of the binder in the active material and the adhesion with the active material can be improved, thereby completing the present invention.

[0013] The present invention is as follows. [1] A powdery binder for a secondary battery positive electrode, comprising a non-crosslinked polymer having a glass transition temperature of 60° C. or higher and 150° C. or lower. [2] The powdery binder for secondary battery positive electrodes according to [1], wherein the non-crosslinked polymer has a structural unit derived from a non-crosslinked ethylenically unsaturated monomer. [3] The powdery binder for a secondary battery positive electrode according to [2], wherein the non-crosslinkable ethylenically unsaturated monomer comprises a non-crosslinkable aromatic vinyl monomer or a non-crosslinkable ethylenically unsaturated carboxylate monomer. [4] The powdery binder for a secondary battery positive electrode according to any one of [1] to [3], wherein the non-crosslinked polymer has a structural unit derived from a non-crosslinked ethylenically unsaturated carboxylic acid monomer in an amount of 5% by mass or less relative to all structural units of the non-crosslinked polymer. [5] The powdery binder for a secondary battery positive electrode according to any one of [1] to [4], wherein the particle size of the non-crosslinked polymer is a volume-based median diameter (D50) of 80 nm to 800 nm as measured by a dynamic light scattering method. [6] A powdery particle composite comprising a positive electrode active material and the powdery binder for a secondary battery positive electrode according to any one of [1] to [5]. [7] A secondary battery positive electrode, comprising a mixture layer formed of the powdery particle composite according to [6] on a surface of a current collector. [8] A secondary battery comprising the secondary battery positive electrode described in [7]. Beneficial Effects

[0014] The powdery binder for a secondary battery positive electrode of the present invention can improve the productivity of the secondary battery positive electrode, and can also improve the dispersibility of the binder in the active material and the adhesion with the active material. DETAILED DESCRIPTION

[0015] The powdered binder for the positive electrode of a secondary battery of the present invention (hereinafter also referred to as "the present binder") contains a non-crosslinked polymer (hereinafter also referred to as "the present non-crosslinked polymer") having a glass transition temperature of 60°C or higher and 150°C or lower. Furthermore, the present binder is used as a powdered particle complex containing a positive electrode active material, and a positive electrode mixture layer is formed on the surface of a current collector such as an aluminum foil by the powdered particle complex, thereby obtaining a positive electrode of the secondary battery of the present invention.

[0016] Here, the "powdered" in the present adhesive means that the solid content concentration is 85% by mass or more, and the determination method of the solid content concentration is described below. In addition, as the solid content concentration, especially in the case of manufacturing anodes for secondary batteries by dry mixing, it is more preferably 90% by mass or more, more preferably 95% by mass or more, further preferably 97% by mass or more, and further preferably 98% by mass or more. (Method for measuring solid content concentration) About 0.5 g of polymer is collected into a weighing bottle whose weight has been measured in advance [weight of weighing bottle = B (g)], and after the weighing bottle and the polymer are correctly weighed [W0 (g)], the polymer and the weighing bottle are placed in a ventilated dryer and dried at 155°C for 45 minutes. The weight at this time is measured together with the weighing bottle [W1 (g)], and the solid content concentration is calculated using the following formula (1). Solid content concentration (%) = (W1-B) / (W0-B) × 100 (1)

[0017] Hereinafter, the elements constituting the present binder will be described together with the powdery particle composite, the secondary battery positive electrode, and the secondary battery containing the present binder will also be described in detail. In the present specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid, "(meth)acrylate" means acrylate and / or methacrylate, and "(meth)acryloyl" means acryloyl and / or methacryloyl. In the numerical ranges recorded in stages in this specification, the upper limit value or lower limit value recorded in one numerical range may be replaced by the upper limit value or lower limit value of the numerical range recorded in other stages, and the upper limit value or lower limit value of the numerical range may also be replaced by the value shown in the embodiment.

[0018] 1. This adhesive The present binder contains the present non-crosslinked polymer, which melts under relatively high temperature compression processing conditions and covers the positive electrode active material. Therefore, the adhesive and the active material can have excellent adhesion. On the other hand, since the glass transition temperature of the present non-crosslinked polymer is above 60°C and below 150°C, the adhesive will not be welded when the powdered particle composite is prepared, and the dispersibility of the adhesive in the active material can be excellent.

[0019] From the viewpoint of being able to improve the dispersibility of the binder in the active material, the glass transition temperature (hereinafter referred to as "Tg") of the present non-crosslinked polymer is preferably 65°C to 150°C, more preferably 70°C to 140°C, further preferably 75°C to 130°C, further preferably 80°C to 130°C, further preferably 85°C to 120°C, and yet further preferably 90°C to 110°C. In addition, in this specification, Tg can be measured by a differential scanning calorimeter (DSC) described in Examples.

[0020] <Structural Unit of the Non-crosslinked Polymer> The non-crosslinked polymer has substantially no structural unit derived from a crosslinkable monomer as a structural unit, and has a structural unit derived from a monomer other than the crosslinkable monomer (hereinafter also referred to as a "non-crosslinkable monomer"). The non-crosslinkable monomer is not particularly limited, but preferably has a structural unit derived from a non-crosslinkable ethylenically unsaturated monomer, and the content of the structural unit is preferably 50% by mass or more and 100% by mass or less, more preferably 60% by mass or more and 100% by mass or less, further preferably 70% by mass or more and 100% by mass or less, and still further preferably 80% by mass or more and 100% by mass or less, relative to all the structural units of the non-crosslinked polymer. Examples of the non-crosslinkable ethylenically unsaturated monomer include non-crosslinkable aromatic vinyl monomers (hereinafter also referred to as "monomer (a1)"), non-crosslinkable ethylenically unsaturated carboxylic acid ester monomers (hereinafter also referred to as "monomer (a2)"), non-crosslinkable ethylenically unsaturated carboxylic acid monomers (hereinafter also referred to as "monomer (a3)"), non-crosslinkable nitrile group-containing ethylenically unsaturated monomers, non-crosslinkable (meth)acrylamide and its derivatives, non-crosslinkable maleimide compounds, and the like. Among them, from the viewpoint of being able to improve the dispersibility of the binder in the active material and the adhesion with the active material, it is preferred to contain a structural unit derived from the monomer (a1) or the monomer (a2).

[0021] <Structural Units Derived from Monomer (a1) and Monomer (a2)>

[0022] Examples of the monomer (a1) include styrene, α-methylstyrene, vinylnaphthalene, isopropenylnaphthalene, and the like. These monomers may be used alone or in combination of two or more. The content of the monomer (a1) component in the present non-crosslinked polymer is not particularly limited, but is preferably 50% by mass or more and 100% by mass or less, more preferably 60% by mass or more and 100% by mass or less, further preferably 70% by mass or more and 100% by mass or less, and still further preferably 80% by mass or more and 100% by mass or less, based on all the structural units of the present non-crosslinked polymer.

[0023] As the monomer (a2), a (meth)acrylate monomer is preferred, and examples thereof include alkyl (meth)acrylate compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; Aromatic (meth)acrylate compounds such as phenyl (meth)acrylate, phenyl methyl (meth)acrylate, phenyl ethyl (meth)acrylate, and phenoxyethyl (meth)acrylate; (Meth)acrylate alkoxyalkyl ester compounds such as 2-methoxyethyl (meth)acrylate and 2-ethoxyethyl (meth)acrylate; Hydroxyalkyl (meth)acrylate compounds such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate may be used alone or in combination of two or more.

[0024] The content of the monomer (a2) component in the present non-crosslinked polymer is not particularly limited, but is preferably 1% by mass or more and 100% by mass or less, more preferably 1% by mass or more and 50% by mass or less, further preferably 1% by mass or more and 30% by mass or less, and still further preferably 1% by mass or more and 20% by mass or less, relative to all structural units of the present non-crosslinked polymer.

[0025] <Structural Unit Derived from Monomer (a3)> Examples of the monomer (a3) ​​include (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid; (meth)acrylamide alkyl carboxylic acids such as (meth)acrylamide caproic acid and (meth)acrylamide dodecanoic acid; succinic acid monohydroxyethyl (meth)acrylate, ω-carboxy-caprolactone mono(meth)acrylate, (meth)acrylate β-carboxyethyl ester, and the like, any one of which may be used alone or in combination of two or more. The amount of the structural unit derived from the monomer (a3) ​​in the non-crosslinked polymer is not particularly limited, and for example, it may contain 15% by mass or less relative to all the structural units of the non-crosslinked polymer. By containing the component (a3) ​​in the above range, the mechanical stability of the non-crosslinked polymer can be improved. It is preferably 13% by mass or less, more preferably 11% by mass or less, further preferably 9% by mass or less, further preferably 7% by mass or less, further preferably 5% by mass or less, and further preferably 3% by mass or less.

[0026] <Other structural units> Examples of other structural units in the non-crosslinked polymer include structural units derived from non-crosslinked nitrile group-containing ethylenically unsaturated monomers, non-crosslinked (meth)acrylamide and derivatives thereof, non-crosslinked maleimide compounds, etc. The amount of the other structural units relative to the total amount of monomers constituting the non-crosslinked polymer is, for example, 50% by mass or less, 30% by mass or less, 10% by mass or less, 5% by mass or less, or 1% by mass or less.

[0027] Examples of the non-crosslinking ethylenically unsaturated monomer containing a nitrile group include: (meth)acrylonitrile; (meth) cyanoalkyl acrylate compounds such as cyanomethyl (meth)acrylate and cyanoethyl (meth)acrylate; cyano group-containing unsaturated aromatic compounds such as 4-cyanostyrene and 4-cyano-α-methylstyrene; 1,1-dicyanodized ethylene (シアンビニリデン); any one of these may be used alone or in combination of two or more.

[0028] Examples of the non-crosslinked (meth)acrylamide derivatives include N-alkyl (meth)acrylamide compounds such as N-isopropyl (meth)acrylamide and N-tert-butyl (meth)acrylamide; N-alkoxyalkyl (meth)acrylamide compounds such as N-n-butoxymethyl (meth)acrylamide and N-isobutoxymethyl (meth)acrylamide; N,N-dialkyl (meth)acrylamide compounds such as N,N-dimethyl (meth)acrylamide and N,N-diethyl (meth)acrylamide; and cyclic (meth)acrylamide compounds such as 4-acryloylmorpholine. Any one of these may be used alone or in combination of two or more.

[0029] Non-crosslinking maleimide compounds include maleimide and N-substituted maleimide compounds. Examples of N-substituted maleimide compounds include N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-ethylmaleimide, N-n-propylmaleimide, N-isopropylmaleimide, N-n-butylmaleimide, N-isobutylmaleimide, N-tert-butylmaleimide, N-pentylmaleimide, N-hexylmaleimide, N-heptylmaleimide, N-octylmaleimide, N-laurylmaleimide, and N-stearylmaleimide; N-cyclopentylmaleimide; , N-cycloalkyl substituted maleimide compounds such as N-cyclohexylmaleimide; N-phenylmaleimide, N-(4-hydroxyphenyl)maleimide, N-(4-acetylphenyl)maleimide, N-(4-methoxyphenyl)maleimide, N-(4-ethoxyphenyl)maleimide, N-(4-chlorophenyl)maleimide, N-(4-bromophenyl)maleimide, N-benzylmaleimide and other N-aryl substituted maleimide compounds, etc., any one of which may be used alone or in combination of two or more.

[0030] <Particle size of the non-crosslinked polymer> The particle size of the non-crosslinked polymer is, from the perspective of excellent adhesion to the active material, a volume-based median particle size (D50) measured by a dynamic light scattering method of, for example, 80 nm to 950 nm, preferably 80 nm to 800 nm, more preferably 80 nm to 750 nm, further preferably 80 nm to 700 nm, further preferably 80 nm to 650 nm, and further preferably 80 nm to 600 nm. In addition, in this specification, the particle size can be measured by the dynamic light scattering method described in the Examples.

[0031] <Method for producing the non-crosslinked polymer> The non-crosslinked polymer can be prepared by a known polymerization method such as solution polymerization, precipitation polymerization, suspension polymerization, emulsion polymerization, etc., and can be appropriately selected according to the molecular weight, composition, etc. The polymerization initiator may be azo compounds, organic peroxides, inorganic peroxides, and other known polymerization initiators, but is not particularly limited. The use conditions may be adjusted by using known methods such as thermal initiation, redox initiation with a reducing agent, and UV initiation to achieve an appropriate amount of free radical generation. Furthermore, for the purpose of adjusting the molecular weight, a known chain transfer agent may be used as necessary.

[0032] Here, emulsion polymerization is preferred among the polymerization methods because a non-crosslinked polymer having the above-mentioned particle size can be obtained and the effects achieved by the present invention are remarkable. As methods of emulsion polymerization, for example, intermittent reaction, dripping reaction, etc. can be cited, wherein the intermittent reaction is to add all the monomers, surfactants, and water into a reaction tank for reaction; the dripping reaction is to slowly drip the monomers into the reaction tank for reaction. Among them, the dripping reaction is preferred in terms of easy control of heat release in the polymerization reaction. In addition, in order to further improve the polymerization stability, the dripping reaction is preferably to mix the monomer, water and surfactant, stir, and drip after forming an emulsified monomer pre-emulsion. At this time, there is a solvent mainly composed of water in the reaction tank. The surfactant is preferably mixed in the solvent. Furthermore, the solvent is preferably preheated, and the heating conditions are, for example, 50°C to 120°C, and 70°C to 100°C.

[0033] The emulsion polymerization is preferably carried out in the presence of at least one of a surfactant and a protective colloid. For the surfactant, anions, cations, and nonions are preferred as ionic species, and anions and nonions are more preferred. In addition, a polymerizable surfactant having an ethylenically unsaturated double bond can also be used.

[0034] Anionic surfactants refer to surfactants that can become ions in aqueous solution and whose hydrophilic part becomes anions. In addition, nonionic surfactants refer to surfactants that do not dissociate into ions in aqueous solution and show surface activity. In addition, cationic surfactants refer to surfactants that can become ions in aqueous solution and whose hydrophilic part becomes cations. Polymerizable surfactants refer to anionic or nonionic surfactants having one or more unsaturated double bonds that can be free radical polymerized in the molecule.

[0035] The above-mentioned surfactants can be used alone or in combination of two or more. There is no particular restriction on the amount of the surfactant, and it is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the monomer mixture (in this specification, "monomer mixture" refers to a mixture containing monomers and chain transfer agents). The use of a suitable amount of surfactant can further improve the mechanical stability of the resin particles, and the use of a suitable amount of polymerizable surfactant can further improve the mechanical stability. When the amount is less than 0.1 parts by mass, it is difficult to ensure the emulsification stability. In addition, when it is greater than 20 parts by mass, the water resistance is significantly reduced.

[0036] It is preferred to use a radical polymerization initiator (hereinafter also referred to as a "polymerization initiator") in the emulsion polymerization. As the polymerization initiator, a known oil-soluble polymerization initiator or water-soluble polymerization initiator can be used. Examples of the oil-soluble initiator include organic peroxides such as benzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl hydroperoxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, and terpene hydroperoxide; and azobis compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and 1,1'-azobis-cyclohexane-1-carbonitrile. Examples of the water-soluble polymerization initiator include ammonium persulfate, sodium persulfate, potassium persulfate, hydrogen peroxide, and 2,2′-azobis(2-methylpropionamidine) dihydrochloride.

[0037] For emulsion polymerization, a reducing agent may be used together with a polymerization initiator. This can promote the polymerization reaction. Examples of such reducing agents include reducing organic compounds such as ascorbic acid, isoascorbic acid, tartaric acid, citric acid, glucose, and metal salts such as formaldehyde sulfoxylate; reducing inorganic compounds such as sodium sulfite, sodium bisulfite, sodium pyrosulfite (SMBS), and sodium hyposulfite; ferrous chloride, sodium formaldehyde sulfoxylate, thiourea dioxide, and the like.

[0038] It is preferred to use a water-soluble polymerization initiator for emulsion polymerization. The polymerization initiator is preferably used in an amount of 0.05 to 5% by mass relative to 100 parts by mass of the monomer mixture. The reducing agent is preferably used in an amount of 0.01 to 2.5% by mass relative to 100 parts by mass of the monomer mixture.

[0039] During emulsion polymerization, a buffer, a chain transfer agent, a basic compound, etc. may be used as needed. Examples of the buffer include sodium acetate, sodium citrate, sodium bicarbonate, etc. Examples of the chain transfer agent include 2-mercaptoethanol, octyl mercaptan, tert-dodecyl mercaptan, lauryl mercaptan, stearyl mercaptan, 2-ethylhexyl thioglycolate, octyl thioglycolate, 2-ethylhexyl mercaptopropionate, octyl mercaptopropionate, etc.

[0040] Furthermore, the present adhesive can be obtained by drying the non-crosslinked polymer obtained by the above-mentioned polymerization method. As a drying method, there is no particular limitation as long as the non-crosslinked polymers can be dried in a state where they can be redispersed without being excessively fused to each other, and examples thereof include a method of drying an aqueous dispersion by a ventilated dryer (e.g., 70° C.), a method of spray drying an aqueous dispersion of a non-crosslinked polymer, a method of drying by a rotary evaporator, and the like. Furthermore, it is more preferred to dry under vacuum after drying by spray drying or rotary evaporator drying.

[0041] The drying temperature is preferably lower than the minimum film-forming temperature of the non-crosslinked polymers from the viewpoint of being able to remove water without excessively fusing the non-crosslinked polymers to each other and enabling redispersion. If the drying temperature is too high, the non-crosslinked polymers will become films and thus be difficult to redisperse.

[0042] In addition, from the viewpoint of being able to dry the non-crosslinked polymer in a redispersible state, the minimum film-forming temperature of the non-crosslinked polymer is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 80° C. or higher. If the minimum film-forming temperature is too low, it becomes difficult to dry the non-crosslinked polymers without excessively fusing them to each other.

[0043] Here, the minimum film-forming temperature is the minimum temperature for forming the film of the above-mentioned non-crosslinked polymer. The minimum film-forming temperature can be measured according to JIS K6828-2 (2003). Specifically, an aqueous dispersion of a non-crosslinked polymer is coated and dried on a flat plate such as an iron plate with an appropriate temperature gradient to a thickness of about 100 μm, and the boundary temperature of the filmized part and the non-filmized part is measured. Here, since the filmized part becomes transparent and the non-filmized part becomes turbid, the boundary between the filmized part and the non-filmized part can be visually confirmed. In addition, when the flat plate after coating and drying the aqueous dispersion of the non-crosslinked polymer is rubbed, the non-filmized part will fall powder (powder falls), so the boundary between the filmized part and the non-filmized part can also be confirmed based on whether there is powder falling.

[0044] 2. Powdered particle complex The powdery particle composite of the present invention contains a positive electrode active material and the present binder. Relative to the total amount of 100 parts by mass of the positive electrode active material, the amount of the present adhesive in the present powdered particle composite is, for example, more than 0.1 parts by mass and less than 10 parts by mass. The above-mentioned amount is also, for example, more than 0.2 parts by mass and less than 8 parts by mass, and is also, for example, more than 0.3 parts by mass and less than 5 parts by mass, and is also, for example, more than 0.4 parts by mass and less than 5 parts by mass. If the amount of the present adhesive is more than 0.1 parts by mass, sufficient adhesion can be obtained. In addition, if the amount of the present adhesive is less than 10 parts by mass, the adhesive is evenly dispersed in the positive electrode active material, and a mixture layer with a uniform and smooth surface can be formed, which is also preferred from the viewpoint of the energy density and resistance of the secondary battery.

[0045] Among the above active materials, lithium salts of transition metal oxides can be used as positive electrode active materials, for example, layered rock salt type and spinel type lithium-containing metal oxides can be used. Specific compounds of layered rock salt type positive electrode active materials include lithium cobalt oxide, lithium nickel oxide, and NCM {Li(Ni x ,Co y , Mn z ), x+y+z=1} and NCA{Li(Ni 1-a-b Co a Al b )}, etc. In addition, as the spinel type positive electrode active material, lithium manganate, etc. can be cited. In addition to oxides, phosphates, silicates and sulfur, etc. are also used. As phosphates, olivine type lithium iron phosphate, etc. can be cited. As the positive electrode active material, one of the above can be used alone, or two or more can be combined as a mixture or a composite.

[0046] From the viewpoint of being able to increase the energy density of the secondary battery, the amount of active material used in the present powdered particle complex is preferably in the range of 70 mass % to 99.9 mass %, more preferably in the range of 80 mass % to 99.9 mass %, and further preferably in the range of 90 mass % to 99.9 mass %, relative to the total amount of the present powdered particle complex.

[0047] Since the electrical conductivity of any positive electrode active material is low, a conductive aid is usually added for use. As the conductive aid, carbon materials such as carbon black, carbon nanotubes, carbon fibers, graphite powder, and carbon fibers can be cited, among which carbon black, carbon nanotubes, and carbon fibers are preferred from the viewpoint of easily obtaining excellent electrical conductivity. In addition, as carbon black, Ketjen black and acetylene black are preferred. The conductive aid can be used alone or in combination of two or more. From the viewpoint of taking into account both electrical conductivity and energy density, the amount of the conductive aid used can be, for example, 0.2 to 20 parts by mass, and can also be, for example, 0.2 to 10 parts by mass, relative to the total amount of 100 parts by mass of the active material. In addition, the positive electrode active material can also use a material that has been surface-coated with a conductive carbon material.

[0048] This powdered particle complex can also be used in combination with other binder components such as styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC) and polyvinylidene fluoride. In the case of using other binder components, the amount used can be, for example, 0.1% by mass to 5% by mass or less, and can also be, for example, 0.1% by mass to 2% by mass or less, and can also be, for example, 0.1% by mass to 1% by mass or less. If the amount of other binder components used is greater than 5% by mass, the resistance increases, and there is a situation where the high rate characteristics are insufficient. From the viewpoint of excellent balance between adhesion and bending resistance, SBR and CMC are preferred among the above, and SBR and CMC are more preferably used in combination.

[0049] The above-mentioned SBR represents a copolymer having a structural unit derived from an aromatic vinyl monomer such as styrene and a structural unit derived from an aliphatic conjugated diene monomer such as 1,3-butadiene. As the above-mentioned aromatic vinyl monomer, in addition to styrene, α-methylstyrene, vinyltoluene, divinylbenzene, etc. can also be cited, and one or more of them can be used. Mainly from the viewpoint of adhesion, the structural unit derived from the above-mentioned aromatic vinyl monomer in the above-mentioned copolymer can be set to a range of, for example, 20% to 70% by mass, and can also be set to a range of, for example, 30% to 60% by mass. As the above-mentioned aliphatic conjugated diene monomer, in addition to 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, etc. can also be cited, and one or more of them can be used. In terms of the good adhesion of the binder and the flexibility of the obtained electrode, the structural unit derived from the above-mentioned aliphatic conjugated diene monomer in the above-mentioned copolymer can be set to a range of, for example, 20% to 70% by mass, and can also be set to a range of, for example, 30% to 60% by mass. In order to further improve the properties such as adhesion, in addition to the above-mentioned monomers, SBR can also use the following monomers as other monomers and as copolymer monomers: (meth) acrylonitrile and other nitrile-containing monomers; (meth) acrylic acid, itaconic acid, maleic acid and other carboxyl-containing monomers; (meth) methyl (meth) acrylate and other ester-containing monomers. The content of the structural unit derived from the other monomer in the copolymer may be, for example, in the range of 0% by mass to 30% by mass, or further in the range of 0% by mass to 20% by mass.

[0050] The above-mentioned CMC represents a nonionic cellulose-based semi-synthetic polymer compound substituted with a carboxymethyl group and a salt thereof. Examples of the above-mentioned nonionic cellulose-based semi-synthetic polymer compound include: alkyl celluloses such as methyl cellulose, methylethyl cellulose, ethyl cellulose, and microcrystalline cellulose; Hydroxyalkyl celluloses such as hydroxyethyl cellulose, hydroxybutyl methyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose stearyl ether, carboxymethyl hydroxyethyl cellulose, alkyl hydroxyethyl cellulose, and nonylphenol polyether hydroxyethyl cellulose.

[0051] The powdered particle composite of the present invention has the above-mentioned positive electrode active material and the present binder as essential components. The mixing method of the components is not particularly limited and a known method can be used. In addition to the above-mentioned components, it is preferably manufactured by dry-mixing powder components such as a conductive aid as needed. In addition, the powdered particle composite of the present invention can be mixed with a dispersion medium such as water and then dispersed and kneaded to produce an electrode slurry. As the dispersion medium, in addition to water, lower alcohols such as methanol and ethanol, carbonates such as ethylene carbonate, ketones such as acetone, tetrahydrofuran, water-soluble organic solvents such as N-methylpyrrolidone, etc. can be cited.

[0052] 3. Secondary battery positive electrode The secondary battery positive electrode of the present invention is an electrode having a composite layer formed by the powdered particle composite of the present invention on the surface of a current collector such as aluminum. For the composite layer, after the powdered particle composite is coated on the surface of the current collector, a compression treatment using mold stamping and roller pressing is implemented. The compression treatment makes the active material and the binder close together, which can improve the strength of the composite layer and the adhesion to the current collector. The compression treatment can, for example, adjust the thickness of the composite layer to about 30% to 80% before the compression treatment, and the thickness of the composite layer after the compression treatment is generally about 4μm to 200μm.

[0053] 4. Secondary battery The secondary battery electrode of the present invention is provided with a secondary battery negative electrode, a separator and an electrolyte, so that a secondary battery can be produced. The electrolyte may be in a liquid state or in a gel state. The separator is arranged between the positive electrode and the negative electrode of the battery, and is responsible for preventing the short circuit caused by the contact between the two poles, maintaining the electrolyte and ensuring the ionic conductivity. For the separator, it is preferred to have a film-like insulating microporous film with good ion permeability and mechanical strength. As a specific material, polyolefins such as polyethylene and polypropylene, polytetrafluoroethylene, etc. can be used.

[0054] In addition, as the negative electrode active material used for the negative electrode of the above-mentioned secondary battery, for example, carbon-based materials, lithium metal, lithium alloys and metal oxides can be cited, and one of them or a combination of two or more thereof can be used. Among them, the negative electrode active material composed of carbon-based materials such as natural graphite, artificial graphite, hard carbon and soft carbon (hereinafter also referred to as "carbon-based negative electrode active material") is preferred, and graphite such as natural graphite and artificial graphite, and hard carbon are more preferred. In addition, in the case of graphite, from the perspective of battery performance, spheroidized graphite is preferably used, and the preferred range of its particle size is, for example, 1μm to 20μm, and also, for example, 5μm to 15μm. In addition, in order to improve the energy density, metals or metal oxides such as silicon and tin that can absorb lithium can also be used as negative electrode active materials. Among them, silicon has a higher capacity than graphite, and negative electrode active materials composed of silicon-based materials such as silicon, silicon alloys and silicon oxides such as silicon monoxide (SiO) (hereinafter also referred to as "silicon-based negative electrode active materials") can be used. However, although the above-mentioned silicon-based negative electrode active material has a high capacity, on the other hand, the volume change accompanying charging and discharging is large. Therefore, it is preferably used in combination with the above-mentioned carbon-based negative electrode active material. In this case, if the amount of silicon-based negative electrode active material is large, it will lead to the collapse of the electrode material, and there is a situation where the cycle characteristics (durability) are greatly reduced. From this point of view, when a silicon-based negative electrode active material is used in combination, its usage amount is, for example, less than 60% by mass, and for example, less than 30% by mass, relative to the carbon-based negative electrode active material.

[0055] The carbon-based negative electrode active material itself has good electrical conductivity, so it is not necessary to add a conductive aid. In the case of adding a conductive aid for the purpose of further reducing resistance, from the viewpoint of energy density, the amount used is, for example, 10% by mass or less, and also, for example, 5% by mass or less, relative to the total amount of the negative electrode active material.

[0056] Regarding the electrolyte, commonly used known electrolytes can be used according to the type of active material. In lithium-ion secondary batteries, specific solvents include: cyclic carbonates with high dielectric constants and high electrolyte solubility such as propylene carbonate and ethylene carbonate; and low-viscosity chain carbonates such as ethyl methyl carbonate, dimethyl carbonate and diethyl carbonate; they can be used alone or as a mixed solvent. Lithium salts such as LiPF6, LiSbF6, LiBF4, LiClO4, and LiAlO4 are dissolved in these solvents and used as electrolytes. In nickel-hydrogen secondary batteries, potassium hydroxide aqueous solution can be used as an electrolyte. A secondary battery can be obtained by making the positive plate and the negative plate separated by a diaphragm into a rolled or laminated structure and storing them in a shell, etc.

[0057] As described above, the secondary battery shows good durability (cycle characteristics) even after repeated charge and discharge, and is therefore suitable for a vehicle-mounted secondary battery or the like, wherein the secondary battery includes an electrode including a mixture layer formed of the powdery particle composite disclosed in this specification. Example

[0058] Hereinafter, the present disclosure will be specifically described based on examples. In addition, the present disclosure is not limited to these examples. In addition, the following "parts" and "%" mean parts by mass and mass % unless otherwise specified. In the following examples, polymers were evaluated by the following methods.

[0059] <Measurement of Particle Size> After 0.02 g of the aqueous dispersion containing the polymer was diluted about 1000 times with 20 g of pure water, the particle size distribution was measured using a particle size analyzer based on the dynamic light scattering method (nanoSAQLA manufactured by Otsuka Electronics Co., Ltd.) to obtain the volume-based median particle size (D50) as a representative value of the particle size.

[0060] <Determination of Glass Transition Temperature> For the polymer, a differential scanning calorimeter (DSC 214 Polyma manufactured by NETZSCH, standard material: alumina) was used, and the heat change point when the temperature was increased from -50°C to 150°C at a rate of 10°C / min was taken as the glass transition temperature.

[0061] <Weldability of polymer after drying at 70°C> A: After drying, the polymer does not fuse but becomes powder B: After drying, the polymer is fused into a film, not a powder

[0062] <Determination of Solid Content Concentration> About 0.5 g of polymer is collected into a weighing bottle whose weight has been measured in advance [weight of weighing bottle = B (g)], and after the weighing bottle and the polymer are correctly weighed [W0 (g)], the polymer and the weighing bottle are placed in a ventilated dryer and dried at 155°C for 45 minutes. The weight at this time is measured together with the weighing bottle [W1 (g)], and the solid content concentration is calculated using the following formula (1). Solid content concentration (%) = (W1-B) / (W0-B) × 100 (1)

[0063] Polymer Manufacturing (Production Example 1: Production of Polymer R-1) In the polymerization, a reactor equipped with a stirring blade, a thermometer, a reflux cooler and a nitrogen inlet pipe was used. Under a nitrogen atmosphere, 50 parts of water were added to the reactor, and the reactor was heated to 70°C. Next, 40 parts of water, 2.0 parts of sodium lauryl sulfate (manufactured by Kao Corporation, trade name "Emaul 2F-30") as a surfactant in terms of solid content equivalent, 95 parts of styrene, 4 parts of 2-ethylhexyl acrylate, and 1 part of methacrylic acid were added to another container equipped with a stirring blade to prepare an emulsified mixed solution. Furthermore, after adding 0.2 parts of ammonium persulfate (hereinafter also referred to as "APS"), which is a polymerization initiator, into the reactor, the emulsified mixed solution was added to the reactor at a constant rate over 3 hours. In addition, a liquid prepared in advance in another container and mixed with 0.2 parts of APS and 10 parts of water was added to the reaction solution at a constant rate over 3 hours. The reaction was continued until the polymerization conversion rate was greater than 98%, and an aqueous dispersion of polymer R-1 was obtained. The particle size of polymer R-1 was 260 nm.

[0064] (Production Examples 2 to 15 and Comparative Production Examples 1 to 2: Production of Polymers R-2 to R-17) Aqueous dispersions of polymers R-2 to R-17 were obtained by the same operation as in Production Example 1 except that the amount of each raw material added was as shown in Table 1. Table 1 shows the measurement results of the particle sizes of polymers R-2 to R-17.

[0065] 《Manufacturing of powdered binder for secondary battery positive electrode》 (Manufacturing Example 1: Manufacture of Powdered Binder R-1 for Secondary Battery Positive Electrode) For the aqueous dispersion of polymer R-1 obtained in Manufacturing Example 1, after drying in a ventilated dryer at 70°C, the polymer was not welded (A evaluation). Furthermore, it was dried in a vacuum dryer at 2kPa, 60°C, and 4 hours. The obtained solid was crushed to obtain a powdered binder R-1 for a secondary battery positive electrode containing polymer R-1. The glass transition point temperature of polymer R-1 is 92°C, and the solid content concentration is 99.2% by mass.

[0066] (Manufacturing Examples 2 to 15 and Comparative Manufacturing Examples 1 to 2: Manufacture of Powdered Binders for Secondary Battery Positive Electrodes R-2 to R-17) The aqueous dispersions of polymers R-2 to R-17 obtained in Manufacturing Examples 2 to 15 and Comparative Manufacturing Examples 1 to 2 were dried in the same manner as in Manufacturing Example 1 to obtain powdered binders for secondary battery positive electrodes R-2 to R-17 containing polymers R-2 to R-17. In addition, the glass transition point temperatures of polymers R-2 to R-17, the evaluation results of the weldability after drying at 70°C, and the solid content concentrations are shown in Table 1.

[0067] [Table 1]

[0068] The details of the compounds used in Table 1 are shown below. St: Styrene HA: 2-Ethylhexyl Acrylate BA: n-butyl acrylate MMA: Methyl methacrylate IBOMA: Isobornyl Methacrylate MAA: Methacrylic acid AN: Acrylonitrile Surfactant 1: 30% aqueous solution of sodium lauryl sulfate (manufactured by Kao Corporation, trade name "Emaul 2F-30") Surfactant 2: 25% aqueous solution of polyoxyethylene styrenated allylphenyl ether ammonium sulfate (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., trade name "Aqualon AR-1025") ·AMA: Allyl methacrylate (cross-linking monomer) ·APS: Ammonium Persulfate

[0069] Example 1 <Evaluation of dispersibility of powdered binder in active material> LiNi as the positive electrode active material is placed in the container. 0.8 Co0.15 Al 0.05 99 parts of O2(NCA) and 1 part of a powdered binder (R-1) containing polymer R-1, and 100 parts of zirconium oxide beads (φ=1 mm) were mixed using a paint shaker for 60 minutes to allow the binder to adhere to the positive electrode active material and disperse it uniformly, thereby obtaining a powdered particle complex. Afterwards, the dispersion state of the binder was visually evaluated. The evaluation results are shown in Table 2.

[0070] (Criteria for evaluating dispersibility in active substances) A: After dispersing the positive electrode active material, no white binder is found B: After the positive electrode active material is dispersed, the white color of the binder can be visually observed, but no lumps (blocks) remain. C: Large clumps of binder remaining after dispersing the positive electrode active material In addition, a rating of B or above is considered a passing level.

[0071] <Evaluation of Adhesion Between Powdered Binder and Active Material> The powdery particle composite obtained above was sandwiched between two pieces of aluminum foil (20 μm, manufactured by UACJ) and subjected to compression treatment at “120° C., 10 minutes, press pressure 3 MPa” or at “150° C., 10 minutes, press pressure 3 MPa”. After the compression treatment, the adhesion between the aluminum foil and the positive electrode active material when the aluminum foil was peeled off was evaluated. The unbonded active material was brushed off 10 times from the compressed aluminum foil with a brush, and the adhesion was evaluated based on the mass of the active material that slipped off. The evaluation results are shown in Table 2. (Criteria for determining adhesion to active material) A: The slippage of active substances is less than 10% B: The amount of active material slipping is 10% or more and less than 30% C: The amount of active material slipping is 30% or more The smaller the amount of active material sliding off, the better the adhesive bonding is, and a rating of B or higher is considered a pass level.

[0072] Example 2 to Example 18 and Comparative Examples 1 to 2 A powdery particle composite was obtained by the same operation as in Example 1 except that the formulation was set as shown in Table 2, and the dispersibility of the powdery binder in the active material and the adhesion with the active material were evaluated.

[0073] [Table 2]

[0074] The details of the compounds used in Table 2 are shown below. NCA: LiNi 0.8 Co 0.15 Al 0.05 O2 (manufactured by BASF Toda Pilot Medical Co., Ltd., trade name "NCA7051") NMC: LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (manufactured by BASF Toda Pilot Medical Co., Ltd., trade name "NCM111 1040") ·AB: Acetylene black (manufactured by Ducon Co., Ltd., trade name "Decon Li-400")

[0075] 《Evaluation Results》 From the results of Examples 1 to 18, it can be seen that by using the powdered binder for secondary battery positive electrodes of the present invention, the positive electrode can be manufactured by dry mixing rather than electrode slurry, so the productivity is excellent, and the powdered binder has excellent dispersibility in the active material and adhesion with the active material. Among them, focusing on the glass transition temperature, the powdered binder has excellent dispersibility in the active material when the glass transition temperature is 70°C or higher (Example 1, Example 14, Example 16, Example 17) compared to the case where the glass transition temperature is 63°C (Example 15). In addition, if the glass transition temperature is in the range of 73°C to 109°C, the adhesion between the powdered binder and the active material is rated B or higher regardless of the compression treatment condition of 120°C or 150°C (Example 1, Example 14, Example 16). Furthermore, focusing on the amount of the structural unit derived from the ethylenically unsaturated carboxylic acid monomer, the case where the amount of the structural unit derived from methacrylic acid was 5 mass % or less (Example 1, Example 10) had better adhesion to the active material than the case where the amount was 10 mass % (Example 11). Furthermore, in addition, focusing on the particle size, if the particle size is in the range of 90nm to 700nm, the adhesion with the active material is excellent under the compression treatment condition of 150°C (Example 1, Example 5 to Example 8), and if the particle size is in the range of 90nm to 510nm, the adhesion with the active material is excellent even under the compression treatment condition of 120°C (Example 1, Example 5 to Example 7).

[0076] In contrast, the adhesion of the powdered binder containing a cross-linked polymer having a structural unit from a cross-linking monomer to the active material is significantly poor (Comparative Example 1). This is believed to be because the cross-linked polymer does not melt under high temperature (120°C and 150°C) compression treatment conditions and does not cover the positive electrode active material. In addition, when the glass transition temperature of the non-cross-linked polymer is less than 60°C (Comparative Example 2), the powdered binder is welded, so the result is that the dispersibility of the powdered binder in the active material is significantly poor. Industrial Applicability

[0077] The powdery binder for a secondary battery positive electrode disclosed in this specification can produce a secondary battery positive electrode by dry mixing without using an electrode slurry, and therefore has excellent productivity, and the powdery binder has excellent dispersibility in an active material and adhesion to the active material. Furthermore, a secondary battery including a secondary battery positive electrode obtained using the powdered binder can ensure good integrity and is expected to show good durability (cycle characteristics) even after repeated charge and discharge, and is therefore expected to contribute to higher capacity of vehicle-mounted secondary batteries and the like. The powdery binder for a secondary battery positive electrode of the present invention can be particularly suitably used for a non-aqueous electrolyte secondary battery positive electrode, and is particularly useful for a non-aqueous electrolyte lithium ion secondary battery having a high energy density.

Claims

1. A powdery binder for a secondary battery positive electrode, in, The powdery binder for a secondary battery positive electrode contains a non-crosslinked polymer having a glass transition temperature of 60° C. or higher and 150° C. or lower.

2. The powdery binder for a secondary battery positive electrode according to claim 1, in, The non-crosslinked polymer has a structural unit derived from a non-crosslinked ethylenically unsaturated monomer.

3. The powdery binder for the secondary battery positive electrode according to claim 2, in, The non-crosslinkable ethylenically unsaturated monomer includes a non-crosslinkable aromatic vinyl monomer or a non-crosslinkable ethylenically unsaturated carboxylate monomer.

4. The powdery binder for a secondary battery positive electrode according to any one of claims 1 to 3, in, The non-crosslinked polymer has 5% by mass or less of a structural unit derived from a non-crosslinkable ethylenically unsaturated carboxylic acid monomer based on all structural units of the non-crosslinked polymer.

5. The powdery binder for a secondary battery positive electrode according to any one of claims 1 to 4, in, The particle size of the non-crosslinked polymer is 80 nm to 800 nm in terms of volume-based median particle size (D50) measured by a dynamic light scattering method.

6. A powdery particle composite, in, The powdery particle composite comprises a positive electrode active material and the powdery binder for a secondary battery positive electrode according to any one of claims 1 to 5.

7. A secondary battery positive electrode, in, The secondary battery positive electrode comprises a mixture layer formed of the powdery particle composite according to claim 6 on the surface of a current collector.

8. A secondary battery, in, The secondary battery comprises the secondary battery positive electrode according to claim 7 .