Method for manufacturing laminated iron core, laminated iron core, and rotating electrical machine using laminated iron core
In the punching process of amorphous metal thin plates, the side with a small surface roughness is used as the punching surface and the number of laminated sheets is appropriately selected, which solves the problems of large mold consumption and short life, and achieves efficient laminated cores Manufacturing and productivity improvements.
Patent Information
- Application Number
- CN202380035384.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-10
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-29
AI Technical Summary
In the punching and processing of existing amorphous metal thin plates, the mold consumption is large and the life is short, which affects productivity and efficiency. The difference in surface roughness leads to uneven mold burden, making it difficult to effectively reduce mold consumption.
By using the side with a small surface roughness as the punching surface, combined with laminated multi-piece amorphous metal thin plates for punching and processing, the friction work and mold wear are reduced, and the number of laminated pieces per unit laminated body is appropriately selected to reduce mold consumption and Risk of damage.
It improves the productivity of punching and processing of amorphous metal thin plates, extends the service life of the mold, reduces the consumption and damage risks of the mold, and achieves efficient laminated core manufacturing.
Smart Images

Figure CN119054183A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a laminated core using an amorphous metal thin plate, the laminated core, and a rotating electric machine using the laminated core. Background Art
[0002] In order to curb global warming, it is required to develop a technology that reduces carbon dioxide (CO2) emissions. Therefore, there are great expectations for high efficiency of motors. About 70% of the electricity used in the industrial field and about 40% of the electricity used in households are consumed by motors. It can be said that by improving the efficiency of each motor by just a few percent, it is possible to expect energy-saving effects equivalent to power plants of hundreds of thousands of kW, which can help reduce millions of tons of CO2 each year. On the other hand, in recent years, electric vehicles have become significantly popular for the purpose of reducing CO2 emissions, and in order to extend the driving distance on a single charge, the demand for improving the efficiency of drive motors has increased.
[0003] Conventional stator cores using electromagnetic steel sheets generally use a die to punch out electromagnetic steel sheets with a thickness of 0.15 mm to 0.5 mm into an annular cross-sectional shape with grooves (slots), and the punched parts are stacked and fixed by riveting, welding, bonding, etc. to form a cylindrical stator core.
[0004] Here, amorphous metals have attracted attention as materials to meet the strong social demand for higher efficiency of motors in recent years. Compared with existing electromagnetic steel sheets, the iron loss of amorphous metals is very small, about 1 / 10. Therefore, if amorphous metals can be used as materials for the cores of stators and rotors for motors, the efficiency can be greatly improved (for example, +5 to 6%) compared to existing motors that use electromagnetic steel sheets for the cores.
[0005] However, in the current manufacture of amorphous metal sheets, the mainstream manufacturing method is a "roller method" in which molten iron-based metal or cobalt-based metal is continuously supplied to a rotating cooling roller and rapidly solidified on the cooling roller. The rotation speed of the cooling roller is adjusted to cool the molten alloy at a predetermined speed to generate a thin strip of amorphous metal sheet. In this roller method, only a thin foil-shaped amorphous metal sheet with a thickness of about 25 μm can be generated. On the other hand, the hardness of amorphous metal sheets (amorphous metal foil) is very high (Hv = about 900 to 1100), which is extremely high compared to ordinary electromagnetic steel sheets (Hv = about 200 to 300). Therefore, when punching an amorphous metal sheet into a stator shape, a mold using a superhard alloy material is used. However, if an amorphous metal sheet with a thickness of about 25 μm is to be used as a raw material for a stator core, the number of times the raw material with a thickness of the amount of a stator core is punched becomes very large. For example, the iron core for motors can be several meters high. If an electromagnetic steel sheet with a thickness of 0.35 to 0.5 mm is used, each one requires thousands to tens of thousands of punching operations. In contrast, if an amorphous metal sheet is used as the raw material for the iron core for motors, the number of times the raw material with the thickness of one iron core is punched increases to 14 to 20 times that of the electromagnetic steel sheet. Furthermore, since the amorphous metal sheet is very hard, the load on the die (punch) increases, so there is a problem that the die life becomes extremely short. In addition, the thickness of the amorphous metal sheet is very thin, so it is sometimes referred to as an amorphous metal sheet below.
[0006] As a technology for solving such technical problems, a technology described in Japanese Patent Publication No. 56-36336 (Patent Document 1) is known. Patent Document 1 discloses a manufacturing method, firstly stacking amorphous metal thin plates with electrical insulating layers therebetween, and then mechanically punching them into a predetermined core shape, thereby manufacturing a stacked core composed of amorphous metal thin plates.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 56-36336 Summary of the invention
[0010] Problems to be solved by the invention
[0011] According to the technique of Patent Document 1, it is described that punching out a plurality of amorphous metal thin plates in a stacked state has an effect of significantly reducing the consumption of the die used, compared with a method of punching out each amorphous metal thin plate.
[0012] However, in the technology of Patent Document 1, there is no description of further significantly reducing the consumption of the die used for punching by taking into account the properties of the amorphous metal thin plate to be punched.
[0013] However, in the case of manufacturing an amorphous metal sheet using the roller method, the difference in properties when comparing the surfaces of both sides of the metal foil, specifically, the surface roughness, is greatly different. The inventors focused on the difference in surface roughness of the amorphous metal sheet and repeatedly conducted a large number of experiments and studies on how this difference affects actual punching. As a result, they obtained the following new discovery: punching from the side with a smaller surface roughness significantly reduces the burden on the die used compared to punching from the side with a larger surface roughness. Therefore, using this new discovery, they challenged new issues such as improving productivity and significantly reducing die consumption compared to the past, and achieved the solution of this technical issue.
[0014] The object of the present invention is to provide a method for manufacturing a laminated iron core, a laminated iron core based on the manufacturing method, and a rotating electric machine using the same, which can significantly reduce the consumption of dies in the punching process of amorphous metal thin plates while improving productivity and achieving a longer life.
[0015] Solutions to Solve Problems
[0016] The present invention lists an example, which is a method for manufacturing a laminated iron core, which uses a mold to punch out an amorphous metal sheet to perform a predetermined shape processing, and uses the amorphous metal sheet after a predetermined amount of shape processing to manufacture the laminated iron core. The shape processing includes the following steps: a step of stacking multiple sheets of the amorphous metal sheet to form a stacked amorphous metal sheet; and a step of placing the surface with a small surface roughness of the stacked amorphous metal sheet on the processing side and then punching it out using the mold.
[0017] In addition, another example of the present invention is a laminated iron core used in electrical equipment, wherein the laminated iron core is formed using a predetermined amount of unit laminates, wherein the unit laminates are formed by stacking multiple amorphous metal thin plates and punching them out in a manner that produces collapsed edges on a surface with a small surface roughness.
[0018] Furthermore, if another example of the present invention is listed, it is a rotating electric machine using a laminated iron core, wherein the laminated iron core is formed using a required number of unit laminates, and the unit laminates are formed by multiple amorphous metal thin plates punched out in a manner that produces collapsed edges on surfaces with less surface roughness.
[0019] Effects of the Invention
[0020] According to the present invention, productivity can be improved and the life of a die used for punching an amorphous metal thin plate can be prolonged. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a figure which shows the cross-sectional shape of the belt-shaped amorphous metal thin plate.
[0022] Figure 2 It is a diagram for explaining the measurement position of the edge shape of the cylindrical punch in the verification experiment.
[0023] Figure 3A This is a diagram showing data when punching an amorphous metal thin plate from the side with greater surface roughness.
[0024] Figure 3B This is a diagram showing data when punching an amorphous metal thin plate from the side with a smaller surface roughness.
[0025] Figure 4 This is a diagram showing a finite element method model of punching of an amorphous metal thin plate.
[0026] Figure 5 This is a diagram showing the relationship between the number of laminated sheets constituting a unit laminate and the friction work per punching sheet.
[0027] Figure 6 This is a graph showing the relationship between the number of laminated sheets and the maximum principal stress of tension on the punch surface.
[0028] Fig. 7A This is a diagram for explaining why the maximum principal stress of tension decreases as the number of laminated sheets increases, and is a diagram showing the case where the number of laminated sheets is 1.
[0029] Figure 7B This is a diagram for explaining why the maximum principal stress of tension decreases as the number of stacked sheets increases, and is a diagram showing the case where the number of stacked sheets is 4.
[0030] Figure 8 This is a graph showing the relationship between the number of laminated sheets per unit laminate and the equivalent compressive stress on the punch surface.
[0031] Fig. 9 It is a diagram showing a laminated core manufacturing system according to the first embodiment of the present invention.
[0032] Fig.10 This is a diagram for explaining the formation of the stacked amorphous metal thin plates in Example 1.
[0033] Fig.11 It is a diagram showing a stator according to a second embodiment of the present invention.
[0034] Fig.12 It is a diagram showing a rotating electrical machine according to a third embodiment of the present invention.
[0035] Fig.13 This is a diagram showing a stator of a rotating electrical machine according to a third embodiment. DETAILED DESCRIPTION
[0036] Hereinafter, the present invention will be described in detail through specific embodiments. In addition, the present invention is not limited to the embodiments (embodiments) described below for explanation, and those skilled in the art can easily understand that the structure can be changed within the scope of the technical idea or purpose of the present invention. In addition, in the following description, the same figure mark (number) is used in principle for the same device, the parts with the same action and function, and repeated descriptions are sometimes omitted. In addition, the position, size, shape, range, etc. of each structure shown in the drawings are simplified for easy understanding of the present invention, and do not represent the actual position, size, shape, range, etc. of each structure.
[0037] [Technical considerations regarding the invention]
[0038] First, before describing specific embodiments of the present invention, consideration of technologies related to the present invention or the principle of the invention that are premises of the embodiments will be described.
[0039] The iron core of a rotating electric machine or transformer usually uses an amorphous metal sheet (amorphous metal foil) manufactured by a roll method. In the roll method, a molten metal, which is a material, is supplied to the surface of a cooling roll rotating at a certain speed, and the molten metal is rapidly cooled and solidified on the cooling roll, thereby generating a long amorphous metal sheet (strip-shaped amorphous metal sheet) with a thickness of about 25 μm. The cross section of the strip-shaped amorphous metal sheet manufactured in this way is shown in FIG. Figure 1 The strip-shaped amorphous metal sheet 1 is manufactured by rapidly solidifying the molten metal on the surface of a cooling roll, so the surface roughness of the non-contact surface of the roll is as large as 2.5 μm or more (when the thickness of the raw material is 25 μm), and the surface of the roll contact becomes a smooth surface with a smaller surface roughness than that. Figure 1 As shown, the strip-shaped amorphous metal thin plate 1 has a surface S1 on the non-contact side with the roller and a surface S2 on the contact side with the roller. Figure 1 In the figure, the cross-sectional shape is described roughly for the sake of understanding, and the accurate cross-sectional shape based on actual measurement data is not described. Figure 1 It is understood that the surface S2 on the side directly contacting the cooling roll is a smooth surface with a small surface roughness, but the surface S1 on the side not contacting the cooling roll has a large surface roughness.
[0040] Experiments and studies have been repeatedly conducted on how the difference in surface roughness of the two surfaces affects the punching process. The results show that the load on the die (punch) is very different when the punching process is performed by placing the surface S1 with larger surface roughness on the punch side (processing side) and conversely when the punching process is performed by placing the surface S2 with smaller surface roughness on the punch side (processing side).
[0041] To verify this, a 25 μm thick amorphous metal sheet was used, using a material SKD11 (yield strength: 1570 N / mm 2 , tensile strength: 1810N / mm 2 , compression strength 2700N / mm 2 ) was used for punching, and the shapes of the edge of the front end of the punch in the initial state and the shape of the edge of the front end of the punch after punching 1800 pieces were measured using a three-dimensional measuring machine, and the results were compared. Figure 2 : is a diagram for explaining the measurement position of the edge shape of the punch in this experiment. Figure 2 In FIG. 1 , the shape viewed from the bottom surface of the punch 12 is indicated by 12A, and the shape viewed from the side surface of the punch is indicated by 12B. The edge shape of the punch 12 is measured at a portion 12C indicated by a circle in the figure.
[0042] The results of this verification experiment are shown in Figure 3A and Figure 3B . Figure 3A The following shows a data example when the surface S1 (surface with greater surface roughness) of the amorphous metal thin plate is set as the processing side (punch side) and punched out with a cylindrical punch. Figure 3B This shows an example of data when the surface S2 (the surface with the smallest surface roughness) of the amorphous metal sheet is used as the processing side and punched out with a punch. Figure 3A and Figure 3B In the figure, the dotted line A0 represents the initial state, and the solid line A1 represents the state after punching 1800 times.
[0043] Compare Figure 3A and Figure 3B It can be seen that when the surface S2 with a small surface roughness is arranged on the punch side (processing side) and punching is performed ( Figure 3B The case where the surface S1 with large surface roughness is arranged on the punch side and blanking is performed ( Figure 3A Compared with the case of punching from a surface with a small surface roughness, the punch is greatly deformed toward the outer peripheral side. This is believed to be because the surface roughness of the amorphous metal foil is large, so the friction force at the contact surface with the punch is large, and the punch is dragged by the amorphous metal foil and plastically deformed. Figure 3BIn the case of , wear of the edge of the punch tip was observed, but no plastic deformation toward the outer peripheral side was observed. This is believed to be because the surface roughness of the amorphous metal foil is small, so the friction force at the contact surface with the punch is small, and the punch is not dragged by the amorphous metal foil and deformed.
[0044] As described above, when the punch is used to perform the punching process on the same material the same number of times, it can be understood that the burden on the punch is small when the surface S2 with a small surface roughness is arranged on the punch side and the punching is performed.
[0045] In order to effectively improve the punching productivity of amorphous metal sheets, it is recommended to overlap (stack) multiple amorphous metal sheets before punching. In this case, by stacking a certain number of amorphous metal foils (amorphous metal sheets), the friction work (W / mm) done by the punch during the punching process of each amorphous metal foil is reduced. 2 · pieces) are reduced, and the effect of reducing the wear of the outer periphery of the punch can be obtained. In the embodiment of the present invention, the punching process is performed based on such a concept.
[0046] To conduct this investigation, first, Figure 4 The finite element method model of punching of an amorphous metal thin plate shown in the figure (a model of punching an amorphous metal thin plate 9 into a stacked body 11 of three sheets using a punch 12 and a die 13) was analyzed. The thickness of the band-shaped amorphous metal thin plate 1 in the model was 25 μm.
[0047] Figure 5 The results of using the model to calculate the friction work of each amorphous metal foil when the number of stacked sheets of amorphous metal sheets is changed and punched are shown in . It can be seen that if the number of stacked sheets is more than 3, the friction work of each amorphous metal foil decreases as the number of stacked sheets increases. However, the number of punchings can be reduced by increasing the number of stacked sheets, but the burden on the mold increases each time the punching is performed. Therefore, it is important to appropriately select the number of stacked sheets per unit stack. Therefore, in the improved embodiment of the present invention, the number of stacked sheets is optimized to minimize the consumption of the mold and the risk of damage to the mold.
[0048] Therefore, using the finite element method model described above, the maximum principal stress of tension generated on the surface of the punch when the number of sheets of the unit laminate is changed is calculated. The results are shown in Figure 6The maximum principal stress of tension is generated at the bottom surface of the punch (the surface opposite to the amorphous metal foil). If the number of sheets of the unit stack is set to more than 2, the tensile strength of the ultrafine particle alloy with the highest strength as the raw material of the punch becomes less than 1900MPa. If it is more than 3 sheets, it saturates at about 1000MPa and becomes the minimum. Therefore, by setting the number of stacked sheets of the unit stack to more than 3 sheets, the maximum principal stress of tension, that is, the risk of notching at the bottom surface of the punch, can be minimized.
[0049] The reason why the maximum principal tensile stress decreases when the number of unit laminates is three or more is considered to be as follows: By increasing the number of unit laminates from one to, for example, four, the deflection δ of the amorphous metal thin plate 9 during punching is reduced. Fig. 7A This shows the case where there is one amorphous metal foil. Figure 7B This shows the case where four amorphous metal foils are stacked. Fig. 7A The deflection δ and Figure 7B The deflection δ is Figure 7B The deflection amount δ is small. As a result, the bottom surfaces of the amorphous metal sheet 9 and the punch 12 are close to horizontal, and the component force in the same direction temporarily decreases. After that, the deflection amount of the amorphous metal foil is approximately constant, and the maximum principal stress of tension converges to the minimum.
[0050] on the other hand, Figure 8 The results of the analysis of the equivalent stress generated on the surface of the punch when the number of sheets in the unit stack is changed are shown. The equivalent stress is generated as a compressive stress on the bottom surface of the punch (the surface opposite to the amorphous metal foil), and increases as the number of stacked sheets increases. Among them, when using the highest strength ultrafine particle alloy as the raw material of the punch, in order to prevent damage caused by compression, the equivalent stress must be below the compressive strength of the ultrafine particle alloy of 6500MPa. Figure 8 As shown, in order to satisfy this condition, the number of laminated sheets per unit laminate needs to be 5 or less.
[0051] These research results show that the number of laminated sheets of a unit laminate that can minimize the risk of punch breakage (chipping) and prevent damage due to compression may be set to any number between 3 and 5.
[0052] Hereinafter, specific embodiments of the present invention based on the above-mentioned “technical considerations regarding the invention” will be described.
[0053] [Example 1]
[0054] First, the first embodiment of the present invention will be described. The first embodiment is a laminated iron core manufacturing system for manufacturing a laminated iron core. Fig. 9The structure of the main part of Example 1 is shown. That is, in manufacturing the laminated iron core, there are steps of punching an amorphous metal thin plate using a die to perform a predetermined shape processing, and manufacturing the laminated iron core using a predetermined amount (the number of sheets required for the iron core) of laminated amorphous metal thin plates after the shape processing. Fig. 9 The system shows the process of punching out the amorphous metal thin plate and processing it into a predetermined shape.
[0055] exist Fig. 9 1A to 1C are amorphous metal sheet coils (hereinafter referred to as coils) formed by winding amorphous metal sheets. The amorphous metal sheets (coils) wound into coils 1A to 1C are drawn out as long strips of material by conveying rollers 3A to 3C. The drawn amorphous metal sheets 2A to 2C are supplied to the stacking bonding section 20. In addition, the arrows in the figure indicate the moving direction (conveying direction) of the material (amorphous metal film).
[0056] The stacked bonding portion 20 is formed by applying an adhesive on a plurality of amorphous metal sheets and stacking and bonding them. In addition, a heat-resistant insulating material is used as the adhesive. The stacked amorphous metal sheets are hereinafter referred to as "stacked amorphous metal sheets". In addition, as described above, when the number of stacked sheets of the stacked amorphous metal sheets 21 is set to any number of 3 to 5 sheets, the number of punching processes is reduced to improve productivity, and the wear of the mold is reduced, thereby reducing the risk of damage to the valuable mold, so it is preferred. In the example of the figure, an example of stacking three amorphous metal sheets is shown. The long strip-shaped stacked amorphous metal sheets 21 are conveyed to the stamping machine 30.
[0057] Fig.10 Indicates the state of an amorphous metal thin plate. Fig.10 (a) shows the cross-sectional shape of the amorphous metal thin plates 2A to 2C drawn out (rolled out) by the conveying rollers 3A to 3C. Fig.10 (b) shows the cross-sectional shape of the laminated amorphous metal thin plates 21 laminated by the laminated adhesive portion 20. Fig.10 It can be seen that when three amorphous metal thin plates are stacked, they are stacked in a manner that the surface roughness is the same from top to bottom. That is, when the surface S2 with the smaller surface roughness of the first amorphous metal thin plate is the upper side, the other stacked amorphous metal thin plates are also stacked with the surface S2 with the smaller surface roughness as the upper side. During punching, the stacked amorphous metal thin plates 21 stacked in this way are punched using the die (punch) of the punching machine 30.
[0058] Among them, Fig. 9In the embodiment, when the long strip-shaped amorphous metal sheet is pulled out from the coils 1A to 1C, it is arranged in a manner to become a surface with the same surface roughness as the amorphous metal sheets 2A to 2C and supplied to the stacking bonding section 20. Therefore, it is not necessary to make the surface consistent when bonding and stacking in the stacking bonding section 20. That is, the surface side (upper surface) of the amorphous metal sheet wound as the coils 1A to 1C is made into the same surface S2 with small surface roughness. Therefore, in the stacking bonding section 20, an adhesive is applied to the three amorphous metal sheets 2A to 2C and they are directly stacked and bonded. The upper surface of the stacked stacked amorphous metal sheet 21 becomes the surface S2 with small surface roughness, and the long strip-shaped stacked amorphous metal sheet 21 is directly conveyed to the stamping machine 30. The stamping machine 30 can directly punch out the conveyed stacked amorphous metal sheet 21.
[0059] The punching machine 30 punches out a plurality of stacked amorphous metal sheets 21 (three stacked sheets in this example) into a predetermined shape. In the punching machine 30, an upper die (punch) is installed on a slide that can move up and down. The slide on which the upper die is installed moves up and down along the slide guide by a slide drive mechanism (crank mechanism, a motor driving the crank mechanism, etc.). Thus, the punch moves up and down, and can punch out the stacked amorphous metal foil 21 conveyed to the punching machine. In addition, in this figure, the punching structure and description of the slide, slide drive mechanism, slide guide, etc. are omitted. In addition, the detailed structure and operation description of the upper die (punch) and the lower die (die) constituting the die are also omitted. Among them, the punching process usually performs multiple punching operations. Therefore, it is preferred to use a punching machine suitable for efficiently performing multiple punching operations. As the punching machine 30 used in this embodiment, a punching machine suitable for sequential conveying processing such as a multi-station punching machine is used. Alternatively, a tandem type press machine is used in which a plurality of press machines are arranged in the processing and conveying direction.
[0060] The dies 31 and 32 of the punching machine 30 are composed of an upper die (punch) and a lower die (die), and the upper die is mounted on a slide. When the slide descends, the punch of the upper die punches the material into a predetermined shape. In addition, in the punching machine 30, a structure equipped with two dies 31 and 32 is shown, but three or more dies can be equipped as needed according to the content of the processing.
[0061] The laminated amorphous metal sheets punched and processed into a predetermined shape by the punching machine 30 are transported to the outside of the punching machine 30 by a conveying device not shown. The punched laminated amorphous metal sheets are used as unit laminates of the laminated iron core in the assembly process of the laminated iron core. Therefore, the punched laminated amorphous metal sheets are referred to as "unit laminates" herein.
[0062] The unit stack 40 punched out in this way has a collapsed edge at the end of the surface S2 with a small surface roughness, and burrs on the opposite side (the surface with a large surface roughness). That is, when punching from the surface S2 with a small surface roughness using a punch, the front end of the punch presses the upper surface S2 of the material and presses into the material, initially producing a collapsed edge with an R portion. By further lowering the punch, the punch becomes unable to withstand bending, and the punch will sink into the material and cut the material. Moreover, when the punch is pressed and cut, the material is plastically deformed and protruding burrs are produced. In addition, burrs are usually removed before the assembly process for reasons such as the risk of injury due to sharpness and the risk of poor assembly dimensional accuracy and adverse effects on product performance due to the presence of burrs.
[0063] Next, the unit laminated body 40 formed as the unit laminated body after shape processing is used in the assembly process of the laminated core to manufacture the laminated core. In this assembly process, the unit laminated body 40 is stacked in a predetermined amount (the number of sheets required for the core) and fixed to manufacture the laminated core. In addition, the detailed description of the assembly process is omitted.
[0064] By using such a manufacturing system, it is possible to efficiently produce laminated iron cores used in electrical equipment such as iron cores for transformers and iron cores for stators of rotating electrical machines.
[0065] As described above, in the laminated iron core manufacturing system shown in the first embodiment of the present invention, it is possible to reduce the consumption of the die used in the punching process performed by the punching machine, extend the service life, and improve productivity. Furthermore, since the number of stacked sheets of the stacked amorphous metal thin plates formed before the punching process is set to the number of stacked sheets without the risk of die damage, it is possible to realize an optimal laminated iron core manufacturing method with low die consumption, low risk of die damage, and high productivity.
[0066] [Example 2]
[0067] Next, use Fig.11 Embodiment 2 of the present invention is described. Embodiment 2 shows a stator of a rotating electric machine manufactured using a unit laminate 40 punched out by the method described in Embodiment 1. In this example, an example of a unit laminate 40 formed by stacking four sheets of laminated amorphous metal thin plates 21 and punching them out is shown. In addition, as described above, the number of laminated sheets is preferably set to any number of 3 to 5 sheets.
[0068] exist Fig.11 In the embodiment, the stator 50 is completed by winding coils (not shown) in slots 52 of a laminated core 51 (iron core). Fig.11As shown in the figure on the right side of the drawing by blowing out a part and enlarging it, a required number of unit laminates 40 punched out into a shape for a stator are stacked and assembled by bonding them. The outer peripheral end of the unit laminate 40 is punched out from the surface with less roughness, so that a collapsed edge 41 is formed on the surface with less surface roughness (upper side in the figure).
[0069] According to the second embodiment of the present invention described above, since the unit stack 40 formed by punching out stacked amorphous metal sheets from the side with less surface roughness into the shape of the stator is used for manufacturing, the consumption of the mold is small, the risk of mold damage is low, and the manufacturing of the optimal stator with high productivity can be achieved.
[0070] In addition, in the second embodiment, the stator of the rotating electric machine is described, but the rotor can also be manufactured. In addition, the iron core for the transformer can be manufactured by the same method as in the second embodiment. In this case, of course, the shape of the unit laminated body 40 punched by the punching machine is punched into a shape for the laminated iron core of the transformer. By stacking the necessary amount of unit laminated bodies 40 and bonding them, the laminated iron core of the transformer can be manufactured.
[0071] [Example 3]
[0072] Next, use Fig.12 as well as Fig.13 A third embodiment of the present invention will be described. In the third embodiment, a rotating electrical machine (motor) is manufactured using the laminated core 51 described in the second embodiment. Fig.12 The schematic structure of the rotating electrical machine is shown as a whole. Fig.13 Indicates the part of the stator.
[0073] exist Fig.12 as well as Fig.13 In the embodiment, the motor 100 has a rotor 60 installed around a rotating shaft 70 and a stator 50 installed on the outer periphery of the rotor. The rotor 60 rotates by the electromagnetic action of the stator and the rotor by supplying power from the electric wire 80. The stator 50 uses the stator 50 manufactured in the above-mentioned embodiment 2. Fig.13 As shown, the stator 50 is completed by winding the coils 53 on the slots 52 of the laminated core 51 formed by laminating the unit laminated bodies 40 .
[0074] According to the third embodiment of the present invention described above, since the unit stack 40 for the stator is punched out from the stacked amorphous metal sheets punched out from the side with less surface roughness, the consumption of the mold is small, the risk of mold damage is small, and the rotating motor can be manufactured using a stator with high productivity.
[0075] Explanation of symbols
[0076] 1—strip-shaped amorphous metal sheet, 9—amorphous metal sheet, 12—punch, 13—die, 1A~1C—coil, 2A~2C—amorphous metal sheet, 3A~3C—conveying roller, 20—laminated bonding portion, 21—laminated amorphous metal sheet, 30—stamping machine, 31, 32—die, 40—unit laminate, 41—collapsed edge, 50—stator, 51—laminated iron core, 52—slot, 53—coil, 60—rotor, 70—rotating shaft, 80—wire, 100—motor.
Claims
1. A method for manufacturing a laminated iron core, wherein an amorphous metal thin plate is punched out by a die to perform a predetermined shape processing, and the laminated iron core is manufactured using the amorphous metal thin plate after a predetermined amount of shape processing, wherein the method for manufacturing a laminated iron core is characterized in that: The shaping process includes the following steps: a step of stacking a plurality of the amorphous metal thin plates to form a stacked amorphous metal thin plate; and A step of placing the surface with less surface roughness of the stacked amorphous metal thin plates on the processing side and then performing punching using the die.
2. The method for manufacturing a laminated core according to claim 1, wherein: The number of the laminated amorphous metal thin plates is any number between 3 and 5.
3. The method for manufacturing a laminated core according to claim 1, wherein: The amorphous metal sheet is a long strip-shaped material.
4. The method for manufacturing a laminated core according to claim 1, wherein: The laminated core is an iron core for a stator of a rotating electric machine.
5. A laminated core for use in electrical equipment, the laminated core being characterized in that: The laminated core is formed using a predetermined number of unit laminates, each of which is formed by laminating a plurality of amorphous metal thin plates and punching the laminate so that a collapsed edge is generated on a surface with a small surface roughness.
6. The laminated core according to claim 5, characterized in that The number of laminated sheets of the unit laminate is any number between 3 and 5 sheets.
7. The laminated core according to claim 5, characterized in that The laminated core is an iron core used in a rotating electric machine.
8. The laminated core according to claim 5, characterized in that: The laminated core is an iron core used in a transformer.
9. A rotating electrical machine using a laminated core, wherein: The laminated core is formed using a required number of unit laminates, each of which is formed of a plurality of amorphous metal thin plates punched out so that a collapse occurs on a surface with a small surface roughness.
10. The rotating electrical machine according to claim 9, characterized in that The number of laminated sheets of the unit laminate is any number between 3 and 5 sheets.