Method for manufacturing wiring substrate, method for evaluating resist layer or wiring substrate, and wiring substrate
In the process of manufacturing the wiring substrate, the adhesiveness between the copper plating layer and the seed layer is optimized by using resist layer and electrolytic plating technology, and the problem of copper plating layer collapse is solved, and high-quality fine wiring manufacturing is achieved.
Patent Information
- Application Number
- CN202380035263.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-10
- Filing Date
- 2023-08-09
- Publication Date
- 2024-11-29
AI Technical Summary
When manufacturing a wiring substrate with a copper-plated layer having a width of less than 10 μm, the adhesion between the seed layer and the copper-plated layer is insufficient, resulting in the copper-plated layer being easily collapsed, affecting the stability of the fine wiring.
By providing a resist layer on the seed layer, exposing and developing to form an opening, electrolyzing the copper plating layer, and determining the black portion occupancy ratio (BP occupancy ratio) of the copper plating layer is 45% or less through a specific process to improve the Adhesion between the copper plating layer and the seed layer. The resist layer comprises a binder polymer, a photopolymerizable component and a photopolymerization initiator, especially a 2,4,5-triaryl imidazole dimer derivative, optimizing the formation of the copper plating layer.
The adhesion between the copper plating layer and the seed layer is significantly improved, the risk of the copper plating layer collapse in the etching liquid is reduced, and the stability and quality of the fine wiring are ensured.
Smart Images

Figure CN119054419A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a wiring board, a method for evaluating a resist layer or a wiring board, and a wiring board. Background Art
[0002] In order to cope with the requirements of miniaturization, lightness and high speed of electronic equipment, the wiring substrate constituting the electronic equipment needs to have wiring with a small width. As a method for forming wiring with a small width, semi-additive (SAP) method and modified semi-additive (MSAP) method are widely used (patent document 1). These methods generally include a process of forming a copper plating layer on a seed layer by electrolytic plating. The seed layer is usually formed by electroless plating in SAP and is formed by the stacking of copper foil in MSAP.
[0003] Previous technical literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2004-6773
[0006] Patent Document 2: International Publication No. 2022 / 054873 Summary of the invention
[0007] Technical issues to be solved by the invention
[0008] In the case of forming fine wiring on a seed layer by a copper-plated layer including a portion having a width of less than 10 μm, sometimes the adhesion between the seed layer and the copper-plated layer is insufficient. For example, when removing unnecessary portions of the seed layer by an etching solution, the copper-plated layer (wiring) may collapse easily. One aspect of the present invention relates to a technology that improves the adhesion between the seed layer and the copper-plated layer when manufacturing a wiring substrate by the following method, wherein the method includes a process of forming a copper-plated layer including a portion having a width of less than 10 μm on a seed layer by electrolytic plating.
[0009] Means for solving technical problems
[0010] The present invention includes at least the following means.
[0011] [1] A method for manufacturing a wiring board, the method comprising the following steps:
[0012] providing a resist layer on a seed layer provided on a main surface of a substrate and containing a metal;
[0013] forming a pattern including an opening through which the seed layer is exposed on the resist layer by exposing and developing the resist layer; and
[0014] forming a copper plated layer including a portion having a width less than 10 μm on the seed layer exposed in the opening by electrolytic plating,
[0015] The copper plating layer is formed so that the occupancy rate of the black portion observed in the cross section of the metal portion including the seed layer and the copper plating layer in the width direction of the copper plating layer, that is, the BP occupancy rate is 45% or less,
[0016] The BP occupancy rate is a value determined by the following method, which includes the following steps:
[0017] Finding the number n of black portions observed in a region having a width of L [μm] in a direction parallel to the main surface of the substrate in a cross section of the metal portion including the copper plating layer having a width of less than 10 μm;
[0018] The maximum width w of each of the n black portions in a direction parallel to the main surface of the substrate is obtained. i [μm]; and
[0019] The BP occupancy rate was calculated according to the following formula:
[0020] [Formula 1]
[0021]
[0022] [2] The method according to [1], wherein:
[0023] The method further comprises the following steps:
[0024] removing the resist layer to expose a portion of the seed layer not covered by the copper plating layer; and
[0025] The exposed portion of the seed layer is removed by an etching solution to form a wiring substrate including the wiring having the seed layer and the copper plating layer and the substrate.
[0026] [3] The method according to [1] or [2], wherein:
[0027] The resist layer includes a binder polymer, a photopolymerizable component, and a photopolymerization initiator, and is selected so that the BP occupancy is 45% or less.
[0028] [4] The method according to [3], wherein:
[0029] The photopolymerization initiator includes a 2,4,5-triarylimidazole dimer derivative.
[0030] [5] The method according to [4], wherein:
[0031] The content of the 2,4,5-triarylimidazole dimer derivative in the resist layer is selected within a range of 6 parts by mass or more and 12 parts by mass or less based on 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component.
[0032] [6] The method according to any one of [3] to [5], wherein
[0033] The photopolymerizable component includes a photopolymerizable compound having an oxyalkylene group.
[0034] [7] A method for evaluating a resist layer, the method comprising the following steps:
[0035] providing a resist layer on a seed layer provided on a main surface of a substrate and containing a metal;
[0036] forming a pattern including an opening for exposing the seed layer on the resist layer by exposing and developing the resist layer;
[0037] forming a copper plated layer including a portion having a width less than 10 μm on the seed layer exposed in the opening by electrolytic plating; and
[0038] determining a BP occupancy rate, which is a occupancy rate of a black portion observed in a cross section of a metal portion including the seed layer and the copper plating layer in a width direction of the copper plating layer,
[0039] The method for determining the BP occupancy rate includes the following steps:
[0040] Finding the number n of black portions observed in a region having a width of L [μm] in a direction parallel to the main surface of the substrate in a cross section of the metal portion including the copper plating layer having a width of less than 10 μm;
[0041] The maximum width w of each of the n black portions in a direction parallel to the main surface of the substrate is obtained. i [μm]; and
[0042] The BP occupancy rate was calculated according to the following formula:
[0043] [Formula 2]
[0044]
[0045] [8] A method for evaluating a wiring board, the wiring board comprising a substrate and wiring provided on the substrate, wherein:
[0046] The wiring includes a seed layer provided on the substrate, and a copper plating layer formed on the seed layer and including a portion having a width less than 10 μm,
[0047] The method includes the step of determining a BP occupancy rate, which is a occupancy rate of a black portion observed in a cross section of the wiring in a width direction of the copper plating layer.
[0048] The method for determining the BP occupancy rate includes the following steps:
[0049] Finding the number n of black portions observed in a region having a width of L [μm] in a direction parallel to the main surface of the substrate in a cross section of the wiring including the copper plating layer having a width of less than 10 μm;
[0050] The maximum width w of each of the n black portions in a direction parallel to the main surface of the substrate is obtained. i [μm]; and
[0051] The BP occupancy rate was calculated according to the following formula:
[0052] [Formula 3]
[0053]
[0054] [9] A wiring board comprising:
[0055] substrate; and
[0056] wiring, arranged on the substrate,
[0057] The wiring includes a seed layer provided on the substrate, and a copper plating layer formed on the seed layer and including a portion having a width less than 10 μm,
[0058] The occupancy rate of the black portion observed in the cross section of the wiring in the width direction of the copper plating layer, that is, the BP occupancy rate is 45% or less,
[0059] The BP occupancy rate is a value determined by the following method, which includes the following steps:
[0060] Finding the number n of black portions observed in a region having a width of L [μm] in a direction parallel to the main surface of the substrate in a cross section of the wiring including the copper plating layer having a width of less than 10 μm;
[0061] The maximum width w of each of the n black portions in a direction parallel to the main surface of the substrate is obtained. i [μm]; and
[0062] The BP occupancy rate was calculated according to the following formula:
[0063] [Formula 4]
[0064]
[0065] Effects of the Invention
[0066] When a wiring board is manufactured by a method including forming the copper plating layer on the seed layer by electrolytic plating, the adhesion between the seed layer and the copper plating layer can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 This is a process diagram showing an example of a method for manufacturing a wiring board.
[0068] Figure 2 This is a process diagram showing an example of a method for manufacturing a wiring board.
[0069] Figure 3 This is a cross-sectional view showing an example of a region observed in order to determine the BP occupancy in the cross section of the metal portion.
[0070] Figure 4 This is an example of a scanning electron microscope image of a cross section of a metal portion.
[0071] Figure 5 Yes Figure 4 A partial binarization image of the metal part in the scanning electron microscope image.
[0072] Figure 6 This is a graph showing the relationship between the peel strength of the copper plating layer and the number density of the black portion (BP number density).
[0073] Figure 7 It is the peel strength of the copper plating layer and the average area S of the black part m of the relationship between .
[0074] Figure 8 It is the total peel strength of the copper plating layer and the black part S total of the relationship between .
[0075] Fig. 9 This is a graph showing the relationship between the peel strength of the copper plating layer and the BP occupancy rate. DETAILED DESCRIPTION
[0076] The present invention is not limited to the following examples. In this specification, "(meth)acrylic acid" means both "methacrylic acid" and "acrylic acid". Other similar terms also have the same meaning.
[0077] Figure 1 and Figure 2 This is a process diagram showing an example of a method for manufacturing a wiring board. Figure 1 and Figure 2The method shown includes the following steps in sequence: forming a seed layer 20 including a metal on one main surface 1S of a plate-like substrate 1; providing a resist layer 3 including a resist material on a surface 20S of the seed layer 20 opposite to the substrate 1; forming a pattern including an opening 3A for exposing the seed layer 20 on the resist layer 3 by exposing and developing the resist layer 3; forming a copper plating layer 21 on the seed layer 20 by electrolytic plating; removing the resist layer 3 to expose a portion of the seed layer 20 not covered by the copper plating layer 21; and removing the exposed portion of the seed layer 20 to form a wiring substrate 10 having a wiring 2 having the seed layer 20 and the copper plating layer 21 and a substrate 1. The wiring 2 is formed by removing a portion of the seed layer 20 not covered by the copper plating layer 21 from a metal portion 25 composed of the seed layer 20 and the copper plating layer 21.
[0078] The substrate 1 may be a plate-like body capable of supporting the wiring 2. The outermost layer of the substrate 1 on the side where the seed layer 20 is provided is usually mainly composed of an insulating layer. The insulating layer provided as the outermost layer of the substrate 1 may be, for example, an insulating resin layer such as a buildup. The substrate 1 may include wiring connected to the wiring 2.
[0079] The seed layer 20 is a layer containing metal and is provided for electrolytic plating. The seed layer 20 may be, for example, a metal plating layer formed by electroless plating, a metal foil such as copper foil, a metal layer formed by evaporation such as sputtering, or a metal sintered layer. The metal sintered layer is a layer formed by heating a coating containing metal particles to sinter the metal particles. The seed layer 20 may, for example, contain at least one metal selected from the group consisting of copper, gold, silver, tungsten, molybdenum, tin, cobalt, chromium, iron, zinc, nickel and titanium. The seed layer 20 may be a single layer or may be composed of more than two layers. The thickness of the seed layer 20 may, for example, be more than 100 nm or more than 200 nm, or less than 2000 nm or less than 1000 nm.
[0080] When observing the cross section of the metal part 25 (or wiring 2) composed of the seed layer 20 and the copper-plated layer 21 with a scanning electron microscope, a tiny black part is sometimes observed. Typically, the black part is distributed near the interface between the seed layer 20 and the copper-plated layer 21. The inventor speculates that the black part is a certain defective part such as a tiny pore, which is related to the adhesion between the copper-plated layer 21 and the seed layer 20. It is believed that the black part is mainly caused by a trace amount of resist layer remaining on the seed layer. According to the inventor's opinion, there is a tendency that if the occupancy rate of the black part of the copper-plated layer 21 in the width direction (the direction parallel to the main surface 1S of the substrate 1) is small, the adhesion between the copper-plated layer 21 and the seed layer 20 becomes higher. The number of black parts may also affect the adhesion, especially in the case of fine wiring, the influence of the occupancy rate of the black part is greater than the number of black parts. Hereinafter, this occupancy rate is sometimes referred to as the BP occupancy rate, and is determined by the method described below.
[0081] Figure 3 This is a cross-sectional view showing an example of a region observed in order to determine the BP occupancy in the cross section of the metal portion 25 . Figure 4 This is an example of a scanning electron microscope image of a cross section of a metal portion. Figure 5 Yes Figure 4 A partial binarization image of the metal part in the scanning electron microscope image. Figure 4 The scanning electron microscope image also includes a portion of the insulating resin layer constituting the substrate located below the metal portion. Figure 5 , an enlarged view of a black portion 30i is also shown. The method for determining the BP occupancy rate includes the following steps: finding the number n of black portions 30 observed by a scanning electron microscope in a region R having a width of L [μm] in a direction X parallel to the main surface 1S of the substrate 1 in the cross section of the metal portion 25; finding the maximum width w of each of the n black portions 30 in the direction X i [μm]; and according to the following formula:
[0082] [Formula 5]
[0083]
[0084] Calculate the BP occupancy. The BP occupancy can be determined in two or more regions R, and their average value can be obtained. When n black portions are marked with integer numbers i from 1 to n, the maximum width w of each black portion 30i is i is the maximum width of the black portion 30i with number i. The maximum width wi may be the width of the black portion with number i when the black portion is observed from a direction perpendicular to the direction X (the thickness direction of the substrate 1). The maximum thickness t of each black portion 30i in the thickness direction of the substrate 1 (the direction perpendicular to the direction X) is i Usually less than 0.3 μm.
[0085] In the case where the electrolytic plating layer 21 and the wiring 2 include a portion having a width W of less than 10 μm, the BP occupancy can be determined by observing the black portion in a region having a width of L [μm] in a direction parallel to the main surface 1S of the substrate 1 in a cross section of the metal portion 25 including the copper plating layer 21 having a width of less than 10 μm. The BP occupancy in the cross section of the copper plating layer 21 including a portion having a width of less than 10 μm may greatly affect the adhesion between the copper plating layer 21 and the seed layer 20. If the BP occupancy is large, for example, when an unnecessary portion of the seed layer is removed by an etching solution, a large hole is formed from the black portion, and as a result, the fine wiring may collapse.
[0086] If the BP occupancy is 45% or less, the adhesion between the copper plating layer 21 and the seed layer 20 can be particularly significantly improved. From the same point of view, the BP occupancy can be 40% or less or 35% or less. The BP occupancy can be 0% or more, 5% or more, 10% or more, 15% or more, 20% or more, or 25% or more. A BP occupancy of 0% means that substantially no black portion is observed.
[0087] The copper-plated layer 21 can be formed in such a manner that the BP occupancy is within a specified range (for example, less than 45%). For example, by selecting the resist layer in such a manner that the BP occupancy is within a specified range, a wiring substrate showing high adhesion between the copper-plated layer 21 and the seed layer 20 can be easily obtained. In addition, the resist layer can be evaluated based on the BP occupancy. For example, whether the resist layer is good can be determined based on whether the BP occupancy is within a specified range (for example, less than 45%). An example of a structure of a resist layer that easily provides a low BP occupancy will be described later.
[0088] The wiring board can also be evaluated based on the BP occupancy rate. In this case, for example, whether the wiring board is good or not can be determined based on whether the BP occupancy rate in the cross section of the wiring is within a predetermined range (for example, 45% or less).
[0089] The resist layer 3 can be formed of a photosensitive resist material and may have a thickness of, for example, 5 μm to 120 μm, 5 μm to 50 μm, 10 μm to 120 μm, or 10 μm to 50 μm.
[0090] The resist layer 3 is formed by forming a resist material into a film. The resist material (or the resist layer 3 before exposure) may be, for example, a photosensitive resin composition containing a binder polymer, a photopolymerizable component containing a compound having an ethylenically unsaturated bond, and a photopolymerization initiator.
[0091] The binder polymer may be, for example, an acrylic polymer containing (meth)acrylic acid and (meth)acrylic acid ester as monomer units. The ratio of the monomer units derived from (meth)acrylic acid in the acrylic polymer may be 5 to 30% by mass, 5 to 25% by mass, or 10 to 25% by mass, based on the mass of the acrylic polymer.
[0092] The acrylic polymer may be a copolymer comprising (meth)acrylic acid and benzyl (meth)acrylate or its derivative as monomer units, a copolymer comprising (meth)acrylic acid and styrene or a styrene derivative as monomer units, or a copolymer comprising (meth)acrylic acid, benzyl (meth)acrylate or its derivative and styrene or a styrene derivative as monomer units. The acrylic polymer comprising these monomer units may further comprise an alkyl (meth)acrylate as a monomer unit.
[0093] Specific examples of the benzyl (meth)acrylate derivative constituting the acrylic polymer include 4-methylbenzyl (meth)acrylate, 4-ethylbenzyl (meth)acrylate, 4-tert-butylbenzyl (meth)acrylate, 4-methoxybenzyl (meth)acrylate, 4-ethoxybenzyl (meth)acrylate, 4-hydroxybenzyl (meth)acrylate, and 4-chlorobenzyl (meth)acrylate. The acrylic polymer may contain two or more benzyl (meth)acrylates as monomer units, or may contain both benzyl (meth)acrylate and its derivatives as monomer units.
[0094] The ratio of the monomer unit derived from benzyl (meth)acrylate or a derivative thereof in the acrylic polymer may be 50 to 80 mass %, 50 to 75 mass %, 50 to 70 mass % or 50 to 65 mass % based on the mass of the acrylic polymer.
[0095] Specific examples of styrene derivatives constituting acrylic polymers include vinyltoluene, p-methylstyrene, p-chlorostyrene, α-methylstyrene, p-hydroxystyrene, p-methoxystyrene, p-carboxystyrene and p-(2-chloroethyl)styrene. The acrylic polymer may contain two or more styrene derivatives as monomer units, or may contain both styrene and its derivatives as monomer units.
[0096] The ratio of the monomer unit derived from styrene or a styrene derivative in the acrylic polymer may be 5 to 40% by mass or 5 to 35% by mass based on the mass of the acrylic polymer.
[0097] The (meth)acrylic acid alkyl ester constituting the acrylic polymer may be an ester compound formed by (meth)acrylic acid and a linear or branched aliphatic alcohol having 1 to 12 carbon atoms. The aliphatic alcohol may have 1 to 8 carbon atoms or 1 to 4 carbon atoms. Specific examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. The (meth)acrylic acid alkyl ester constituting the acrylic polymer may have a hydroxyl group. Specific examples of the (meth)acrylic acid alkyl ester having a hydroxyl group include 2-hydroxyethyl (meth)acrylate. The acrylic polymer may contain two or more (meth)acrylic acid alkyl esters as monomer units.
[0098] The ratio of the monomer unit derived from the alkyl (meth)acrylate in the acrylic polymer may be 1 to 20 mass %, 1 to 15 mass %, 1 to 10 mass % or 1 to 5 mass % based on the mass of the acrylic polymer.
[0099] The weight average molecular weight (Mw) of the binder polymer (or acrylic polymer) may be 20000 to 150000, 30000 to 100000, 40000 to 80000, or 40000 to 60000. The weight average molecular weight herein refers to a standard polystyrene conversion value determined by gel permeation chromatography (GPC).
[0100] The acid value (mgKOH / g) of the binder polymer may be 13 to 78, 39 to 65, or 52 to 62. The acid value herein refers to the amount (mg) of potassium hydroxide required to neutralize 1 g of the binder polymer.
[0101] The content of the binder polymer (or acrylic polymer) in the resist material (or the resist layer 3 before exposure) may be 40 to 80 parts by mass, 45 to 75 parts by mass, or 50 to 70 parts by mass based on 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component.
[0102] Specific examples of photopolymerizable components include bisphenol A (meth) acrylate compounds, hydrogenated bisphenol A (meth) acrylate compounds, polyalkylene glycol (meth) acrylates, urethane monomers, pentaerythritol (meth) acrylates, and trimethylolpropane (meth) acrylates. These can be used alone or in combination of two or more. The bisphenol A (meth) acrylate compound can be, for example, a compound represented by the following general formula (1A).
[0103]
[0104] In formula (1A), two Rs are independently hydrogen atoms or methyl groups. EO is oxyethylene, and PO is oxypropylene. m1, m2, n1, and n2 are independently 0 to 40, m1+m2 is 1 to 40, and n1+n2 is 0 to 20. The bonding order of EO and PO is not limited, and either may be located on the (meth)acryloyl side.
[0105] The polyalkylene glycol (meth)acrylate may be a compound represented by the following formula (1B).
[0106]
[0107] In formula (1B), two Rs each independently represent a hydrogen atom or a methyl group, EO represents an oxyethylene group, PO represents an oxypropylene group, s represents 1 to 30, r1 and r2 each independently represent 0 to 30, and r1+r2 is 1 to 30. Examples of commercially available products of the compound represented by formula (1B) include a compound in which R is a methyl group, r1 is a methyl group, r2 is a propylene group, and r3 is a propylene group. 1 +r 2 =4 (average value), s=12 (average value) (manufactured by ShowaDenko Materials Co., Ltd., product name: FA-023M).
[0108] The photopolymerizable component in the resist material (or the resist layer 3 before exposure) may include a photopolymerizable compound having an oxyalkylene group. The resist material including the photopolymerizable compound having an oxyalkylene group can contribute to the reduction of the BP occupancy. For example, the content of the photopolymerizable compound having an oxyalkylene group may be 35 parts by mass or more, 40 parts by mass or more, 45 parts by mass or more, 50 parts by mass or more, or 55 parts by mass or less, or 65 parts by mass or less, or 60 parts by mass or less, relative to the total amount of 100 parts by mass of the binder polymer and the photopolymerizable compound. The photopolymerizable compound having an oxyalkylene group may be, for example, a bisphenol A-based di(meth)acrylate compound represented by formula (1A), a polyalkylene glycol (meth)acrylate represented by formula (1B), or a combination thereof.
[0109] Specific examples of the photopolymerization initiator include aromatic ketones such as benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), N,N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1; 2-ethylanthraquinone, phenanthrenequinone, 2-tert-butylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 2-methylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthrenequinone, 2-methyl-1,4-naphthoquinone, and 2, Quinones such as 3-dimethylanthraquinone; benzoin ether compounds such as benzoin methyl ether, benzoin ethyl ether and benzoin phenyl ether, benzoin, methyl benzoin and ethyl benzoin; benzyl derivatives such as benzyl dimethyl ketal, 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer. At least one 2,4,5-triaryl imidazole dimer derivative selected from the group consisting of 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane, N-phenylglycine, N-phenylglycine derivatives and coumarin compounds. These may be used alone or in combination of two or more. The photopolymerization initiator may include a 2,4,5-triaryl imidazole dimer derivative, and in particular, may include 2-(O-chlorophenyl)-4,5-diphenyl imidazole dimer. The addition of a 2,4,5-triaryl imidazole dimer derivative may contribute to a reduction in BP occupancy.
[0110] The 2,4,5-triarylimidazole dimer derivative is represented by, for example, the following formula (2).
[0111]
[0112] In formula (2), Ar 1 ,Ar 2 and Ar 3 Each independently represents an aryl group (for example, a phenyl group) which may have a substituent. 1 ,Ar 2 or Ar 3 Examples of the substituent that the aryl group may have include a halo group (eg, a chloro group, a fluoro group) and an alkoxy group (eg, a methoxy group). 1 The aryl group may have a substituent.
[0113] The content of the photopolymerization initiator in the resist material (or the resist layer 3 before exposure) can be 0.01 to 5 parts by mass, 0.1 to 4.5 parts by mass, or 1 to 4 parts by mass relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component. The content of the 2,4,5-triaryl imidazole dimer derivative in the resist material (or the resist layer 3 before exposure) can be 5 parts by mass or more, 6 parts by mass or more, 7 parts by mass or more, or 8 parts by mass or less, 12 parts by mass or less, 11 parts by mass or less, 10 parts by mass or less, 9 parts by mass or less, 8.5 parts by mass or less, or 8 parts by mass or less. The content of the photopolymerization initiator (especially the 2,4,5-triaryl imidazole dimer derivative) within an appropriate range can not only improve the sensitivity, resolution and adhesion of the resist material, but also contribute to the improvement of the shape of the pattern formed by the resist layer 3.
[0114] The resist material (or the resist layer 3 before exposure) may contain a dye. The dye may be, for example, at least one selected from the group consisting of a leuco dye, phthalocyanine green, crystal violet, methyl orange, Nile Blue 2B, Victoria Blue, malachite green, methyl green (Basic Blue 20) and diamond green. The leuco dye may be, for example, leuco crystal violet, a fluorane dye or a combination thereof. Leuco crystal violet can also function as a hydrogen donor.
[0115] The content of the dye can be 0.01 to 20 parts by mass relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component. The content of the leuco dye can be 0.1 parts by mass or more and 0.5 parts by mass or more, or 0.1 parts by mass or more and 0.4 parts by mass or more, or 0.1 parts by mass or less and 0.3 parts by mass or less, relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component. The content of malachite green can be 0.05 parts by mass or less, 0.04 parts by mass or less, 0.03 parts by mass or less, or 0.02 parts by mass or more, relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component. The content of leuco dye and malachite green may affect the BP occupancy.
[0116] The resist material (or the resist layer 3 before exposure) may contain other components as needed. Examples of other components include sensitizers, polymerization inhibitors, and adhesive components. The content of other components may be about 0.01 to 20 parts by mass relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component. The adhesive component may include, for example, 5-amino-1H-tetrazole. The content of the adhesive component may affect the BP occupancy.
[0117] The total content of the binder polymer, photopolymerizable component and photopolymerization initiator in the resist material (or the resist layer 3 before exposure) can be 90 to 100% by mass or 95 to 100% by mass relative to the total mass of the components other than the solvent in the resist material (resist layer 3).
[0118] To form the resist layer 3 , a resist film containing a resist material may be stacked on the seed layer 20 , or a resist material containing a solvent may be applied on the seed layer 20 and the solvent may be removed from the applied film.
[0119] A portion of the resist layer 3 is exposed, and the exposed resist layer 3 is developed to form a resist layer 3 having a pattern including an opening 3A. Exposure and development can be performed by a common method known to those skilled in the art. A fine pattern including an opening 3A for exposing the seed layer 20 is formed by exposure through a photomask. The developer used for development may be an alkaline aqueous solution such as an aqueous sodium carbonate solution. The conditions for development may also be selected in such a way that the BP occupancy rate is less than 45%. For example, there is a tendency that if the development time (the contact time between the resist layer and the developer) is long, the BP occupancy rate decreases. The temperature of the developer may be, for example, 20 to 40°C.
[0120] After forming a pattern of the resist layer 3 including the opening 3A and before electrolytic plating, pretreatment can be performed by bringing the surface 20S of the seed layer 20 exposed in the opening 3A into contact with a pretreatment liquid at a specified pretreatment temperature. For the pretreatment liquid adjusted to the specified pretreatment temperature, the surface of the seed layer 20 can be pretreated by immersing an intermediate structure having a substrate 1, a seed layer 20, and a resist layer 3 having a pattern in the pretreatment liquid. The conditions for the pretreatment can be selected in such a way that the BP occupancy is less than 45%. For example, the temperature of the pretreatment liquid can be in the range of 20 to 50°C. The immersion time in the pretreatment liquid can be, for example, more than 1 minute or more than 2 minutes, or less than 8 minutes.
[0121] The pretreatment liquid may be, for example, an acidic aqueous solution containing an acid component, an electrolytic plating additive, and a reducing agent.
[0122] The acid component may be an organic acid, an inorganic acid, or a combination thereof. Specific examples thereof include sulfuric acid; alkanesulfonic acids such as methanesulfonic acid and propanesulfonic acid; alkanolsulfonic acids such as isethionic acid and propanolsulfonic acid; carboxylic acids such as citric acid, tartaric acid, and formic acid. These may be used alone or in combination of two or more. The concentration of the acid component in the pretreatment solution may be 10 to 300 g / L or 50 to 200 g / L based on the volume of the pretreatment solution.
[0123] The additive for electrolytic plating may be, for example, a polyether compound, an organic sulfur compound, or a combination thereof. Examples of polyether compounds include polyethylene glycol, polypropylene glycol, and derivatives thereof. Organic sulfur compounds are copper plating precipitation accelerators sometimes referred to as brighteners, and examples thereof include 3-mercaptopropanesulfonic acid and disodium bis(3-sulfopropyl) disulfide. The concentration of the additive in the pretreatment solution may be 0.1 to 10,000 mg / L based on the volume of the pretreatment solution.
[0124] Examples of reducing agents include hypophosphites, phosphites, dimethylamine borane, trimethylamine borane, hydrazine derivatives, borohydride salts, aldehyde compounds (e.g., formalin, glyoxylic acid), titanium trichloride, catechol, resorcinol, hydroquinone, ascorbate, phenylenediamine, and phosphinic acid derivatives. These can be used alone or in combination of two or more. The concentration of the reducing agent in the pretreatment solution can be 0.0001 to 0.1 mol / L based on the volume of the pretreatment solution.
[0125] The pretreatment liquid may further contain a surfactant selected from alkylbenzene sulfonate and a compound having an acetylene group. The pretreatment liquid may contain a carboxylic acid or an alkanesulfonic acid, an inorganic acid selected from hydrochloric acid, sulfuric acid, phosphoric acid and nitric acid, an alkylbenzene sulfonate and a compound having an acetylene group. In this case, the content of the carboxylic acid and the alkanesulfonic acid may be 5 to 50 g / L or 10 to 20 g / L based on the volume of the pretreatment liquid, and the content of the inorganic acid may be 1 to 20 g / L or 2 to 10 g / L based on the volume of the pretreatment liquid.
[0126] Alkylbenzene sulfonate is a salt of a sulfonic acid compound having a benzene ring, an alkyl group bonded to the benzene ring, and a sulfonic acid group. The number of carbon atoms in the alkyl group can be 10 to 16. The alkylbenzene sulfonate can be a sodium salt, a potassium salt, or a triethanolamine salt. As a specific example of the alkylbenzene sulfonate, linear sodium dodecylbenzene sulfonate can be cited. The content of the alkylbenzene sulfonate can be 0.5 to 20 g / L based on the volume of the pretreatment liquid.
[0127] Commercially available examples of surfactants containing compounds having an acetylene group include Surfynol 104, Surfynol 440, and Surfynol 465 (product names, manufactured by Nissin Chemical Industry Co., Ltd.) The content of the compound containing an acetylene group may be 0.1 to 5 g / L or 0.3 to 1 g / L based on the volume of the pretreatment liquid.
[0128] The pretreatment liquid may contain a dispersant. The dispersant may be a polymer containing a monomer unit derived from maleic acid, and an example of a commercial product thereof may be MALIALIM AKM-0531 (product name, manufactured by NOF CORPORATION). The content of the dispersant may be 0.1 to 5 g / L or 0.3 to 1 g / L based on the volume of the pretreatment liquid.
[0129] Before the electrolytic plating, the surface 20S of the seed layer 20 exposed in the opening 3A may be treated by plasma. The plasma treatment can also contribute to the reduction of the BP occupancy.
[0130] A copper plating layer 21 filling the opening 3A is formed on the surface of the pre-treated seed layer 20 by electrolytic plating. Thereafter, the resist layer 3 is peeled off from the seed layer 20. The seed layer 20 exposed by the peeling of the resist layer 3 is removed by a common method such as etching. As a result, a wiring 2 consisting of the remaining seed layer 20 and the metal plating layer 21 is formed on the substrate 1.
[0131] The electrolytic plating layer 21 and the wiring 2 may include a linear portion, and the width W of the linear portion may be, for example, less than 20 μm, less than 15 μm, less than 10 μm, less than 10 μm, less than 9 μm, less than 8 μm, less than 7 μm, less than 6 μm, less than 5 μm, less than 5 μm or less than 4.9 μm, or more than 1 μm, more than 2 μm, more than 3 μm, more than 4 μm or more than 5 μm. The width W described herein represents the width in a direction perpendicular to the length direction of the linear portion. There is a tendency that if the width W is small, the adhesion between the copper plating layer 21 and the seed layer 20 is more closely related to the BP occupancy rate, for example, compared with the number of black portions. It is believed that the reason is that, for example, there is a tendency that if the width W of the copper plating layer 21 is small, the size of the individual black portion becomes larger.
[0132] Example
[0133] The present invention is not limited to the following examples.
[0134] 1. Resist film
[0135] Resist films 1 and 2 were prepared, each containing the components shown in Table 1 and having a 19 μm thick resist layer and protective films provided on both sides thereof. The table shows the content (parts by mass) of each component relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component.
[0136] [Table 1]
[0137]
[0138] The details of each component shown in the table are as follows.
[0139] (A) Binder polymer
[0140] Acrylic polymer 1: copolymer of methacrylic acid, styrene, benzyl methacrylate, methacrylic acid and methyl methacrylate
[0141] Acrylic polymer 2: copolymer of methacrylic acid, styrene, benzyl methacrylate and 2-hydroxyethyl methacrylate
[0142] (B) Photopolymerizable component
[0143] Monomer A: polyoxyethylene bisphenol A dimethacrylate (compound represented by formula (1A))
[0144] Monomer B: polyoxyalkylene glycol dimethacrylate (compound represented by formula (1B))
[0145] Monomer C: polyoxyethylene bisphenol A dimethacrylate (compound represented by formula (1A))
[0146] (C) Photopolymerization initiator
[0147] B-CIM: 2,2'-bis(o-chlorophenyl)-4,5-4',5'-tetraphenyl-1,2'-biimidazole
[0148] (D) Sensitizer
[0149] ·DBA:9,10-Dibutoxyanthracene
[0150] ·EAB: 4,4'-bis(diethylamino)benzophenone
[0151] (E) Dye
[0152] ·LCV: Leuco Crystal Violet
[0153] MKG: malachite green
[0154] 2. Fabrication of wiring board
[0155] Patterning of resist layer
[0156] A support substrate having a laminate as a prepreg and a substrate provided on the support substrate with an insulating resin layer are prepared. A seed layer (electroless copper plating layer, thickness of about 0.5 μm) is formed on the insulating resin layer. The resist film 1 or 2 with one side of the protective film removed is stacked on the seed layer in a direction so that the resist layer is in contact with the seed layer. Next, the resist layer on the seed layer is exposed via a negative photomask. After exposure, the protective film is peeled off and developed using a 1.0% sodium carbonate aqueous solution as a developer, thereby forming a pattern including a linear opening with a width of 7 μm on the resist layer. The seed layer is exposed in the opening. For development, an ultra-high pressure rotary developing device (manufactured by Blue Ocean Technology., Ltd.) with a spray nozzle is used, and it is carried out by spraying for a time (development time) of 1.5 MD, 1.7 MD or 2 MD based on the developer and then spraying for 100 seconds based on pure water. The developing temperature was 30°C, the rotation speed was 500 rpm, the spray pressure was 0.18 MPa, the moving distance of the spray nozzle head was 7.2 cm, and the moving speed of the spray nozzle head was 10 cm / s. The "MD" of the developing time indicates the ratio of the minimum developing time required to remove the unpatterned resist layer.
[0157] Preprocessing
[0158] For pretreatment, the laminate consisting of the insulating substrate, the seed layer, and the resist layer having the opening was immersed in an acidic pretreatment solution (a 100 mL / L aqueous solution of PB-242D manufactured by JCU CORPORATION, at 45° C.) for 1 minute or 3 minutes. Then, the laminate was immersed in pure water at 50° C. for 1 minute, in pure water at 25° C. for 1 minute, and in a 10% sulfuric acid aqueous solution at 25° C. for 1 minute.
[0159] Electrolytic plating
[0160] The pretreated laminate was immersed in an electrolytic plating solution at a current density of 10 A / dm at 25°C. 2Under the conditions of , a copper plating layer was formed on the seed layer over 10 minutes. As the electrolytic plating solution, a mixed solution of 120 g / L of copper sulfate pentahydrate, 7.3 L of an aqueous solution of 220 g / L of 96% sulfuric acid, 0.25 mL of hydrochloric acid, 92 mL of Top Lucina NSV-1 (product name, OKUNO CHEMICAL INDUSTRIES CO., LTD.), 11.5 mL of Top Lucina NSV-2 (product name, OKUNO CHEMICAL INDUSTRIES CO., LTD.), and 23 mL of Top Lucina NSV-3 (product name, OKUNO CHEMICAL INDUSTRIES CO., LTD.) was used. After the copper plating layer was formed, the laminate was immersed in pure water at room temperature for 1 minute, and the laminate after immersion was dried. The resist layer was stripped by immersing it in a stripping solution (CleanEtch R100 / R100S (Mitsubishi Gas Chemical Company, Inc.)) at 60° C. for 3 minutes to obtain evaluation laminates #1 to #7 having a metal portion including a seed layer and a copper plating layer. Table 2 shows the production conditions of each laminate.
[0161] 3. Evaluation
[0162] 3-1. Black part
[0163] By using a focused ion beam device (Hitachi High-Tech Science Corporation system, MI4050) to process the evaluation laminate, the seed layer is exposed near the interface of the copper plating layer, so as to make a test piece with a cross section roughly parallel to the thickness direction of the evaluation laminate. Using a scanning electron microscope (Hitachi High-Tech Science Corporation system, SU8200), in a plane parallel to the thickness direction of the test piece and perpendicular to the cross section of the test piece, the cross section of the test piece is observed from the direction of 30 ° formed with the thickness direction of the test piece, and photographed with a magnification of 50000 times. The region with a width L of 7 μm in the direction parallel to the main surface of the substrate in the metal portion in the obtained cross-sectional photo is binarized so that the tiny black portion observed only near the interface of the seed layer and the copper plating layer becomes black. For binarization, image editing software ImageJ was used.
[0164] In the binarized image, the number of black areas n and the area S of the individual black areas were calculated. i (i=1 to n) and the maximum width w of a single black portion in a direction parallel to the main surface of the substrate iBased on the obtained values, the number of black portions per 1 μm width of the copper plating layer (BP number density, count / μm) and the average area S of the black portions were calculated according to the following formula: m (μm 2 ), the total area S of the black part of the copper plating layer per 1 μm width total (μm 2 The results are shown in Table 2.
[0165] [Formula 6]
[0166]
[0167] [Table 2]
[0168]
[0169] 3-2. Peel strength
[0170] The peel strength (N / mm) between the copper-plated layer with a width of 7 μm and the seed layer was measured by using a SAICAS N-05 model (product name, DAIPLA WINTES CO., LTD.) and a peel test of cutting and peeling the copper-plated layer with a tiny diamond blade. The measurement conditions are as follows. Two measurements were performed, and the average value of the peel strengths obtained was calculated.
[0171] Measurement mode: Constant speed mode
[0172] Horizontal speed: 1000nm / sec
[0173] Vertical speed: 100nm / sec
[0174] Front angle: 20°, rear angle: 10°
[0175] Figure 6 , Figure 7 , Figure 8 and Fig. 9 They represent the peel strength and BP number density, S m , S total The BP occupancy and the peel strength show the best correlation. In particular, it is confirmed that the peel strength increases significantly when the BP occupancy is 45% or less.
[0176] Explanation of symbols
[0177] 1-substrate, 2-wiring, 3-resist layer, 10-wiring substrate, 20-seed layer, 20S-surface of the seed layer opposite to the substrate, 21-copper plating layer, 25-metal part, 30-black part, wi-maximum width of the black part, W-width of the copper plating layer and the wiring.
Claims
1. A method for manufacturing a wiring substrate, the method comprising the following steps: providing a resist layer on a seed layer provided on a main surface of a substrate and containing a metal; forming a pattern including an opening through which the seed layer is exposed on the resist layer by exposing and developing the resist layer; and forming a copper plated layer including a portion having a width less than 10 μm on the seed layer exposed in the opening by electrolytic plating, The copper plating layer is formed so that the occupancy rate of the black portion observed in the cross section of the metal portion including the seed layer and the copper plating layer in the width direction of the copper plating layer, that is, the BP occupancy rate is 45% or less, The BP occupancy rate is a value determined by the following method, which includes the following steps: Finding the number n of black portions observed in a region having a width of L [μm] in a direction parallel to the main surface of the substrate in a cross section of the metal portion including the copper plating layer having a width of less than 10 μm; The maximum width w of each of the n black portions in a direction parallel to the main surface of the substrate is obtained. i [μm]; and The BP occupancy rate was calculated according to the following formula: [Formula 1] 2. The method according to claim 1, wherein: The method further comprises the following steps: removing the resist layer to expose a portion of the seed layer not covered by the copper plating layer; and The exposed portion of the seed layer is removed by an etching solution to form a wiring substrate including the wiring having the seed layer and the copper plating layer and the substrate.
3. The method according to claim 1 or 2, wherein: The resist layer includes a binder polymer, a photopolymerizable component, and a photopolymerization initiator, and is selected so that the BP occupancy is 45% or less.
4. The method according to claim 3, wherein: The photopolymerization initiator includes a 2,4,5-triarylimidazole dimer derivative.
5. The method according to claim 4, wherein: The content of the 2,4,5-triarylimidazole dimer derivative in the resist layer is selected within a range of 6 parts by mass or more and 12 parts by mass or less relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable component.
6. The method according to claim 3, wherein: The photopolymerizable component includes a photopolymerizable compound having an oxyalkylene group.
7. A method for evaluating a resist layer, the method comprising the following steps: providing a resist layer on a seed layer provided on a main surface of a substrate and containing a metal; forming a pattern including an opening for exposing the seed layer on the resist layer by exposing and developing the resist layer; forming a copper plated layer including a portion having a width less than 10 μm on the seed layer exposed in the opening by electrolytic plating; and determining a BP occupancy rate, which is a occupancy rate of a black portion observed in a cross section of a metal portion including the seed layer and the copper plating layer in a width direction of the copper plating layer, The method for determining the BP occupancy rate includes the following steps: Finding the number n of black portions observed in a region having a width of L [μm] in a direction parallel to the main surface of the substrate in a cross section of the metal portion including the copper plating layer having a width of less than 10 μm; The maximum width w of each of the n black portions in a direction parallel to the main surface of the substrate is obtained. i [μm]; and The BP occupancy rate was calculated according to the following formula: [Formula 2] 8. A method for evaluating a wiring board, the wiring board comprising a substrate and wiring provided on the substrate, wherein: The wiring includes a seed layer provided on the substrate, and a copper plating layer formed on the seed layer and including a portion having a width less than 10 μm, The method includes the step of determining a BP occupancy rate, which is a occupancy rate of a black portion observed in a cross section of the wiring in a width direction of the copper plating layer. The method for determining the BP occupancy rate includes the following steps: Finding the number n of black portions observed in a region having a width of L [μm] in a direction parallel to the main surface of the substrate in a cross section of the wiring including the copper plating layer having a width of less than 10 μm; The maximum width w of each of the n black portions in a direction parallel to the main surface of the substrate is obtained. i [μm]; and The BP occupancy rate was calculated according to the following formula: [Formula 3] 9. A wiring substrate comprising: substrate; and wiring, arranged on the substrate, The wiring includes a seed layer provided on the substrate, and a copper plating layer formed on the seed layer and including a portion having a width less than 10 μm, The occupancy rate of the black portion observed in the cross section of the wiring in the width direction of the copper plating layer, that is, the BP occupancy rate is 45% or less, The BP occupancy rate is a value determined by the following method, which includes the following steps: Finding the number n of black portions observed in a region having a width of L [μm] in a direction parallel to the main surface of the substrate in a cross section of the wiring including the copper plating layer having a width of less than 10 μm; The maximum width w of each of the n black portions in a direction parallel to the main surface of the substrate is obtained. i [μm]; and The BP occupancy rate was calculated according to the following formula: [Formula 4]