Precious metal catalyst, preparation method and application thereof, and method for synthesizing anti-aging agent IPPD by using precious metal catalyst
By using precious metal catalysts, including platinum and rhenium, the problem of poor yield and purity in the synthesis of anti-aging agent IPPD is solved, efficient production under mild conditions is achieved, production costs and side reactions are reduced, and product quality is significantly improved .
Patent Information
- Application Number
- CN202310649710.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art has problems with unsatisfactory product yield and purity in the synthesis of the anti-aging agent IPPD, and the copper-based catalyst causes residual copper in the product to harm the quality of tire production, and it needs to be carried out under high pressure conditions, so the side reaction is more severe.
The catalyst is prepared by spraying the solution of platinum and rhenium containing compounds onto the support using noble metal catalysts, including support and supported active components, such as platinum and rhenium containing compounds, sprayed onto the support, left to stand, washed and dried in vacuo, and condensed under mild conditions. The hydrogenation reaction is used to generate the anti-aging agent IPPD.
It effectively reduces the occurrence of side reactions, improves product yield and purity, and has mild process conditions, saves energy consumption, reduces production costs, and has strong competitiveness.
Smart Images

Figure BDA0004264678790000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fine chemical industry, and in particular relates to a noble metal catalyst, a preparation method and application thereof, and a method for synthesizing an antioxidant IPPD with a noble metal catalyst. Background Art
[0002] Antioxidant IPPD is a general-purpose excellent antioxidant for natural rubber, synthetic rubber and latex. It has good protection against ozone and flex cracking. It is not only an excellent protective agent against heat, oxygen, light and general aging, but also can inhibit the catalytic aging effect of harmful metals such as copper and manganese on rubber. Antioxidant IPPD can be used in tires, inner tubes, hoses, tapes, industrial rubber products, etc. It is one of the main varieties of p-phenylenediamine antioxidants and is also an excellent variety of antioxidants commonly used in the rubber industry at home and abroad.
[0003] Patent CN106554286A provides a method for continuously preparing paraphenylenediamine antioxidants using precious metal catalysts, wherein the method loads precious metal catalysts into a fixed bed or tower reactor to activate the catalyst. 4ADPA and MIBK (or acetone) are configured into a solution, and the reactor is continuously fed with raw materials and hydrogen for condensation hydrogenation reaction, with a hydrogen-to-oil ratio of 1500 to 4500:1. The condensation hydrogenation reaction liquid is vacuum distilled until no fraction is extracted, and the resulting products are antioxidants 6PPD and IPPD. Although the catalyst provided by this patent has a relatively ideal effect in the preparation of antioxidant 6PPD, there are problems in the preparation of antioxidant IPPD in that the product yield and purity are not ideal.
[0004] At present, the main production process for the synthesis of antioxidant IPPD is to generate products by condensation and hydrogenation in a fixed bed reactor using a copper-based catalyst. Copper-based catalysts will cause a small amount of copper to remain in the product IPPD, which will harm the quality of subsequent tire production. In addition, there are problems such as the reaction must be carried out under high pressure and the ketone-to-alcohol side reaction is relatively violent.
[0005] Therefore, it is necessary to develop a catalyst that can synthesize the antioxidant IPPD under mild conditions with high product purity and yield. Summary of the invention
[0006] Aiming at the deficiencies in the prior art, the present invention provides a method for synthesizing an antioxidant IPPD using a noble metal catalyst.
[0007] To this end, the first aspect of the present invention provides a noble metal catalyst, comprising a carrier and an active component supported on the carrier, wherein the active component comprises platinum and rhenium.
[0008] In some embodiments of the present invention, based on the mass of the carrier, the mass content of platinum is 0.1-3wt%, and the mass content of rhenium is 0.1-3wt%. For example, based on the mass of the carrier, the mass content of platinum can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, 1.8%, 2%, 2.2%, 2.4%, 2.7%, 3wt%, etc.; the mass content of rhenium is 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 1.5%, 1.9%, 2%, 2.2%, 2.4%, 2.7%, 2.9%, 3wt%, etc.
[0009] In some embodiments of the present invention, based on the mass of the carrier, the mass content of platinum is 0.1-1.5 wt %.
[0010] In some embodiments of the present invention, the support comprises activated carbon.
[0011] In some embodiments of the present invention, the specific surface area of the carrier is ≥1000m 2 / g.
[0012] In some embodiments of the present invention, the pore volume of the carrier is 0.5-3.0 g / mL.
[0013] In some embodiments of the present invention, the pore size of the carrier is 0.3-2.5 nm.
[0014] In some embodiments of the present invention, the ash content of the carrier is ≤5%.
[0015] In some embodiments of the present invention, the water absorption rate of the carrier is 50-80%.
[0016] In some embodiments of the present invention, the activated carbon is sulfur-containing activated carbon.
[0017] In some embodiments of the present invention, the mass content of sulfur in the carrier is 0.05-0.8 wt %.
[0018] In the present invention, the sulfur content in the carrier is preferably controlled at 0.05-0.8 wt%. The presence of a small amount of sulfur can prevent the initial activity of the catalyst from being too high, avoid the temperature runaway phenomenon, and facilitate industrial large-scale production operations; if the sulfur content is too high, the catalyst will be poisoned and deactivated.
[0019] The second aspect of the present invention provides a method for preparing the precious metal catalyst described in the first aspect, comprising: preparing a platinum-containing compound solution, adding an oxidant to mix, then spraying it onto a carrier, and letting it stand for 2 to 4 hours; obtaining a platinum-containing carrier; preparing a rhenium compound solution, spraying it onto the platinum-containing carrier, and letting it stand for 2 to 4 hours; washing, and vacuum drying to obtain the precious metal catalyst.
[0020] In some embodiments of the present invention, the platinum-containing compound includes chloroplatinic acid.
[0021] In some embodiments of the present invention, the rhenium-containing compound includes potassium perrhenate.
[0022] In some embodiments of the present invention, the oxidant comprises hydrogen peroxide.
[0023] In some embodiments of the present invention, the mass ratio of the oxidant to the carrier is 1 to 25:100.
[0024] In some embodiments of the present invention, the washing is performed to a pH value of 6-7.
[0025] In some embodiments of the present invention, the vacuum drying is carried out at a temperature of 130 to 140° C. and for a time of 3 to 5 hours.
[0026] The third aspect of the present invention provides the use of the noble metal catalyst described in the first aspect or the noble metal catalyst prepared by the preparation method described in the second aspect in the synthesis of amine antioxidants, especially the antioxidant IPPD.
[0027] The fourth aspect of the present invention provides a method for synthesizing an antioxidant IPPD using a precious metal catalyst, comprising: subjecting acetone and 4-aminodiphenylamine to a condensation hydrogenation reaction under the action of the precious metal catalyst described in the first aspect or the precious metal catalyst prepared by the preparation method described in the second aspect to generate the antioxidant IPPD.
[0028] In some embodiments of the present invention, the feed mass ratio of acetone to 4-aminodiphenylamine is 1:2-3.
[0029] In some embodiments of the present invention, the reaction temperature of the condensation hydrogenation reaction is 70-120° C., and the reaction pressure is 0.6-1.2 MPa.
[0030] In some embodiments of the present invention, the method comprises: loading the precious metal catalyst described in the first aspect or the precious metal catalyst prepared by the preparation method described in the second aspect into a fixed bed reactor, replacing with nitrogen, first introducing hydrogen, then introducing acetone and 4-aminodiphenylamine, and carrying out condensation hydrogenation reaction at a temperature of 70 to 120° C. and a pressure of 0.6 to 1.2 MPa. After the reaction is completed, the antioxidant IPPD is obtained by vacuum distillation.
[0031] Beneficial effects:
[0032] The precious metal catalyst provided by the present invention is used for synthesizing the antioxidant IPPD, which can effectively reduce the occurrence of side reactions, and the yield and purity of the product are both high; and the process conditions are mild, which can save energy consumption and reduce equipment investment, saving production costs, and has strong advantages and competitiveness in the current increasingly fierce market competition. DETAILED DESCRIPTION
[0033] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain this patent in detail and do not limit the scope of protection of the present invention in any way.
[0034] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the raw materials, instruments and equipment used in the following examples, etc., can all be purchased on the market or can be obtained by existing methods; the reagent amounts, unless otherwise specified, are the reagent amounts used in conventional experimental operations; the experimental methods, unless otherwise specified, are all conventional methods.
[0035] The coconut shell activated carbon used in the embodiments and comparative examples of the present invention is coconut shell columnar activated carbon produced by Mulinsen Activated Carbon Jiangsu Co., Ltd., and its specific surface area is 1100m 2 / g, pore volume is 0.5-0.65m 3 / g, ash content is 5%, and water absorption is 65%.
[0036] Example 1
[0037] 0.8 g of chloroplatinic acid was dissolved in 30 ml of dilute hydrochloric acid (2 wt%) to prepare a platinum compound solution, and then 20 ml of hydrogen peroxide was added to prepare a mixed solution. The mixed solution was sprayed on 100 g of coconut shell activated carbon in a sugar coating machine, and the mixture was allowed to stand for 2 hours to obtain platinum-containing coconut shell activated carbon. 0.55 g of potassium perrhenate was dissolved in 15 ml of dilute hydrochloric acid (2 wt%) to prepare a rhenium compound solution. The rhenium compound solution was sprayed on the platinum-containing coconut shell activated carbon in a sugar coating machine, and the mixture was allowed to stand for 2 hours. Then, the mixture was washed with sodium carbonate solution (3 wt%) and sodium bicarbonate solution (3 wt%) for 3 times each, and then washed with sodium phosphite solution (3 wt%) until the pH value was 6-7, and vacuum dried at 130° C. for 4 hours to obtain precious metal catalyst 1#.
[0038] Example 2
[0039] 0.3 g of chloroplatinic acid was dissolved in 20 ml of dilute hydrochloric acid (2 wt%) to prepare a platinum-containing compound solution, and 20 ml of hydrogen peroxide was added to prepare a mixed solution. The mixed solution was sprayed on 100 g of coconut shell activated carbon in a sugar coating machine, and the mixture was allowed to stand for 4 hours to obtain platinum-containing coconut shell activated carbon. 3 g of potassium perrhenate was dissolved in 25 ml of dilute hydrochloric acid (2 wt%) to prepare a rhenium-containing compound solution. The rhenium-containing compound solution was sprayed on the platinum-containing coconut shell activated carbon in a sugar coating machine, and the mixture was allowed to stand for 4 hours. Then, the mixture was washed with sodium carbonate solution (3 wt%) and sodium bicarbonate solution (3 wt%) for 3 times each, and then washed with sodium phosphite solution (3 wt%) until the pH value was 6-7, and vacuum dried at 140° C. for 4 hours to obtain precious metal catalyst 2#.
[0040] Example 3
[0041] 3g of chloroplatinic acid was dissolved in 20ml of dilute hydrochloric acid (2wt%) to prepare a platinum-containing compound solution, and then 20ml of hydrogen peroxide was added to prepare a mixed solution. The mixed solution was sprayed on 100g of coconut shell activated carbon in a sugar coating machine, and the mixture was allowed to stand for 2 hours to obtain platinum-containing coconut shell activated carbon. 4.5g of potassium perrhenate was dissolved in 25ml of dilute hydrochloric acid (2wt%) to prepare a rhenium-containing compound solution. The rhenium-containing compound solution was sprayed on the platinum-containing coconut shell activated carbon in a sugar coating machine, and the mixture was allowed to stand for 2 hours. Then, sodium carbonate solution (3wt%) and sodium bicarbonate solution (3wt%) were used to wash the mixture 3 times each, and then sodium phosphite solution (3wt%) was used to wash the mixture until the pH value was 6-7, and the mixture was vacuum dried at 130°C for 4 hours to obtain precious metal catalyst 3#.
[0042] Comparative Example 1
[0043] 0.3 g of chloroplatinic acid was dissolved in 20 mL of dilute hydrochloric acid (2 wt%) to prepare a platinum compound solution, and then 20 mL of hydrogen peroxide was added to prepare a mixed solution. The mixed solution was sprayed on 100 g of coconut shell activated carbon in a sugar coating machine and allowed to stand for 4 hours. Then, the carbon was washed with sodium carbonate solution (3 wt%) and sodium bicarbonate solution (3 wt%) for 3 times each, and then washed with sodium phosphite solution (3 wt%) until the pH value was 6-7, and dried in vacuo at 140° C. for 4 hours to obtain precious metal catalyst 4#.
[0044] Comparative Example 2
[0045] 3 g of potassium perrhenate was dissolved in 25 ml of dilute hydrochloric acid (2 wt%) to prepare a rhenium compound solution, which was sprayed onto coconut shell activated carbon in a sugar coating machine and allowed to stand for 4 hours; then, the carbon was washed with sodium carbonate solution (3 wt%) and sodium bicarbonate solution (3 wt%) for 3 times each, and then washed with sodium phosphite solution (3 wt%) until the pH value was 6-7, and dried under vacuum at 140°C for 4 hours to obtain precious metal catalyst 5#.
[0046] Catalytic effect evaluation
[0047] The catalysts prepared in Examples 1-3 and Comparative Examples 1-2 and the copper-based catalyst NZF (copper oxide content 25-40 wt%) were respectively used to synthesize the antioxidant IPPD. The gas chromatography analysis results are shown in Table 1.
[0048] The method for synthesizing the catalyst prepared in Example 1-3 and Comparative Example 1-2 to produce the antioxidant IPPD is as follows:
[0049] The catalyst was loaded into a fixed bed reaction device, and nitrogen was filled and replaced in the entire fixed bed reaction system at a pressure of 0.2 MPa. After the reaction system was replaced, the temperature was increased, the pressure was adjusted, and hydrogen was introduced with a flow rate controlled at 60 L / min. A continuous synthesis reaction was carried out under the conditions of a temperature of 110° C., a pressure of 1.0 MPa, and a mass ratio of acetone to 4-aminodiphenylamine of 1:2, and the antioxidant IPPD product was obtained by reduced pressure distillation.
[0050] The method for synthesizing antioxidant IPPD using copper catalyst NZF is as follows:
[0051] The copper-based catalyst NZF is loaded into a fixed-bed reaction device, and nitrogen is filled and replaced with a pressure of 0.2 MPa in the entire fixed-bed reaction system. After the reaction system is replaced, the temperature is increased, the pressure is adjusted, and hydrogen is introduced with a flow rate controlled at 60 L / min. A continuous synthesis reaction is carried out under the conditions of a temperature of 120° C., a pressure of 3.0 MPa, and a mass ratio of acetone to 4-aminodiphenylamine of 1:2, and the antioxidant IPPD product is obtained by reduced pressure distillation.
[0052] Table 1
[0053]
[0054] Note: RT refers to 4-aminodiphenylamine; ketone-alcohol ratio refers to the ratio of acetone to isopropanol in the reaction solution, and isopropanol is a product of the side reaction.
[0055] It can be seen from the above experimental results that the active components of the noble metal catalyst provided by the present invention include both platinum and rhenium, and compared with the catalyst whose active components include only platinum or only rhenium, the product purity and yield are significantly improved. Compared with the copper-based catalyst NZF, the noble metal catalyst provided by the present invention not only obtains higher product purity and yield, but also can react under milder conditions.
[0056] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A noble metal catalyst, characterized in that The noble metal catalyst comprises a carrier and an active component supported on the carrier, wherein the active component comprises platinum and rhenium.
2. The noble metal catalyst according to claim 1, characterized in that Based on the mass of the carrier, the mass content of the platinum is 0.1 to 3 wt%, preferably 0.1 to 1.5 wt%; the mass content of the rhenium is 0.1 to 3 wt%.
3. The noble metal catalyst according to claim 1 or 2, characterized in that The carrier includes activated carbon; Preferably, the specific surface area of the carrier is ≥1000m 2 / g; and / or, the pore volume of the carrier is 0.5-3.0g / mL; and / or, the pore size of the carrier is 0.3-2.5nm; and / or, the ash content of the carrier is ≤5%; and / or, the water absorption rate of the carrier is 50-80%; Preferably, the activated carbon is sulfur-containing activated carbon; more preferably, the mass content of sulfur in the carrier is 0.05-0.8 wt %.
4. The method for preparing a noble metal catalyst according to any one of claims 1 to 3, characterized in that: include: Prepare a platinum compound solution, add an oxidant and mix, then spray it onto a carrier and let it stand for 2 to 4 hours; obtaining a platinum-containing carrier; A rhenium compound solution is prepared, sprayed onto a platinum-containing carrier, and allowed to stand for 2 to 4 hours; the solution is washed and vacuum dried to obtain the noble metal catalyst.
5. The preparation method according to claim 4, characterized in that: The platinum-containing compound includes chloroplatinic acid; and / or, the rhenium-containing compound comprises potassium perrhenate; and / or, the oxidant comprises hydrogen peroxide; And / or, the washing is performed until the pH value is 6 to 7; And / or, the vacuum drying is carried out at a temperature of 130 to 140° C. and for a time of 3 to 5 hours.
6. Use of the noble metal catalyst according to any one of claims 1 to 3 or the noble metal catalyst prepared by the preparation method according to claim 4 or 5 in the synthesis of amine antioxidants, especially the antioxidant IPPD.
7. A method for synthesizing an antioxidant IPPD using a noble metal catalyst, characterized in that: include: Acetone and 4-aminodiphenylamine are subjected to condensation hydrogenation reaction under the action of the noble metal catalyst described in any one of claims 1 to 3 or the noble metal catalyst prepared by the preparation method described in claim 4 or 5 to generate the antioxidant IPPD.
8. The method according to claim 7, characterized in that The feed mass ratio of acetone to 4-aminodiphenylamine is 1:2-3.
9. The method according to claim 7 or 8, characterized in that: The reaction temperature of the condensation hydrogenation reaction is 70-120° C., and the reaction pressure is 0.6-1.2 MPa.
10. The method according to any one of claims 7 to 9, characterized in that: The method comprises: loading the noble metal catalyst described in any one of claims 1 to 3 or the noble metal catalyst prepared by the preparation method described in claim 4 or 5 into a fixed bed reactor, replacing with nitrogen, first introducing hydrogen, then introducing acetone and 4-aminodiphenylamine, and carrying out condensation hydrogenation reaction under the conditions of temperature of 70 to 120° C. and pressure of 0.6 to 1.2 MPa, and obtaining the antioxidant IPPD by vacuum distillation after the reaction is completed.