Graphite oxide-based composite material as well as preparation method and application thereof
By adding potassium permanganate in batches to the graphite oxide production and heating, stirring and spray drying, graphite oxide-based composite materials were prepared, which solved the problems of high manganese ion content and wastewater discharge in wastewater, and achieved excellent purification effect and environmental protection goals.
Patent Information
- Application Number
- CN202310617340.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-12-03
AI Technical Summary
In the existing graphite oxide production methods, the manganese ion content in the wastewater is high, the environmental treatment is difficult, and the environmental protection pressure is high, and a large amount of water is required to terminate the reaction step, resulting in wastewater discharge pollution.
The graphite oxide-based composite material is prepared by adding potassium permanganate in batches and heating the reaction in concentrated acid, followed by adding water and stirring and spray-drying, eliminating the use of nitrate and large amounts of water to terminate the reaction step and reducing wastewater discharge.
The prepared graphite oxide-based composite material exhibits excellent performance in the purification reaction, effectively removes sulfides, reduces preparation costs and wastewater discharge, and solves environmental protection problems.
Smart Images

Figure BDA0004254351180000081 
Figure BDA0004254351180000091
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of graphite oxide materials, and in particular relates to a graphite oxide-based composite material and a preparation method and application thereof. Background Art
[0002] Graphite oxide is an important type of graphite product, which can be used to prepare downstream popular products such as expanded graphite and graphene. At present, the main method of producing graphite oxide is to oxidize graphite with strong oxidants such as potassium permanganate, but the existing method has problems such as high manganese ion content in wastewater, difficult environmental treatment, and high environmental pressure. Summary of the invention
[0003] The purpose of the present disclosure is to provide a graphite oxide-based composite material and a preparation method and application thereof. The graphite oxide-based composite material prepared by the present invention contains elements such as manganese, potassium, and sulfur, and exhibits excellent performance and good purification effect in the reaction process such as purification. The preparation method provided by the present invention does not require the addition of nitrates, and at the same time eliminates the step of terminating the reaction with a large amount of water, thereby solving a series of problems such as wastewater discharge.
[0004] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a graphite oxide-based composite material, the method comprising:
[0005] S1: adding graphite to concentrated acid and adding potassium permanganate in batches to obtain a mixed material;
[0006] S2: After heating the mixed material for reaction, water is added and stirred to obtain a mixed slurry, and the mixed slurry is spray-dried to obtain a graphite oxide-based composite material.
[0007] Optionally, the graphite is one or more of natural flake graphite, natural cryptocrystalline graphite and artificial graphite;
[0008] The graphite has a carbon content of more than 95% by weight, an ash content of less than 1%, and a mesh size of 20 to 200 meshes.
[0009] Optionally, the concentrated acid is selected from one or more of sulfuric acid, nitric acid and perchloric acid;
[0010] A0 is any concentration between M-10% and M+10%, preferably A0 is any concentration between M-5% and M+5%, A0 is the concentration of the concentrated acid, and M is the highest concentration of the analytical pure reagent grade of the concentrated acid.
[0011] Optionally, the mass ratio of the concentrated acid to graphite is (10-200):1, preferably (25-100):1.
[0012] Optionally, the mass ratio of potassium permanganate to graphite is (1-10):1, preferably (3-8):1;
[0013] The mass ratio of potassium permanganate to graphite added in each batch is (0.1-2):1, preferably (0.2-1):1.
[0014] Optionally, the method further comprises:
[0015] In step S1, after adding potassium permanganate, the temperature is controlled to below 40° C., preferably below 30° C., more preferably below 20° C., and stirred for 0.1 to 12 hours; no nitrate is added during the reaction;
[0016] In step S2, the conditions of the heating reaction are: temperature of 30-80°C, reaction time of 0.2-12h; the time of stirring with water is 0.1-6h; the conditions of the spray drying include: inlet temperature of 200-400°C, outlet temperature of 120-300°C, and feed rate of the mixed slurry of 10-10000ml / min, preferably 20-2000ml / min.
[0017] Optionally, the water content of the mixed slurry is 50 to 95% by weight, preferably 70 to 90% by weight;
[0018] The mass ratio of the amount of water added to the amount of graphite added is (10-500):1, preferably (20-250):1.
[0019] The second aspect of the present invention provides a graphite oxide-based composite material prepared by the method provided by the first aspect of the present invention.
[0020] Optionally, the graphite oxide-based composite material contains manganese, potassium, sulfur, carbon and oxygen, and based on the mass of the graphite oxide-based composite material, the manganese content is 20-50% by weight, the potassium content is 5-20% by weight, the sulfur content is 10-40% by weight, and the carbon content is 5-30% by weight;
[0021] The specific surface area of the graphite oxide-based composite material is 200 to 700 m 2 / g, preferably 400 to 600 m 2 / g, the pore volume is 0.5 to 2.0 ml / g, preferably 0.8 to 1.5 ml / g, and the average particle size is 0.5 mm or less, preferably 0.2 mm or less.
[0022] The third aspect of the present invention provides use of the graphite oxide-based composite material according to the second aspect of the present invention in removing sulfides.
[0023] Through the above technical scheme, the graphite oxide-based composite material prepared by the present invention contains elements such as manganese, potassium, and sulfur, and exhibits excellent performance in the reaction process such as purification, and has a good purification effect. The preparation method provided by the present invention adds potassium permanganate in batches, and no nitrate needs to be added during the reaction process, while eliminating the step of terminating the reaction with a large amount of water, and there is no wastewater discharge in the entire preparation process, which solves a series of problems such as wastewater discharge polluting the environment.
[0024] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0025] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0026] A first aspect of the present invention provides a method for preparing a graphite oxide-based composite material, the method comprising:
[0027] S1: adding graphite to concentrated acid and adding potassium permanganate in batches to obtain a mixed material;
[0028] S2: After heating the mixed material for reaction, water is added and stirred to obtain a mixed slurry, and the mixed slurry is spray-dried to obtain a graphite oxide-based composite material.
[0029] The preparation method of the invention adds potassium permanganate to graphite in batches, and no nitrate and hydrogen peroxide need to be added during the reaction, thus eliminating the step of terminating the reaction with a large amount of water. Furthermore, no wastewater is discharged during the entire preparation process, thus solving a series of problems such as environmental pollution caused by wastewater discharge.
[0030] In a specific embodiment of the present invention, the graphite is one or more of natural flake graphite, natural cryptocrystalline graphite and artificial graphite, preferably natural flake graphite;
[0031] The graphite has a carbon content of 95% by weight or more, preferably 99% by weight or more, an ash content of 5% or less, preferably 1% or less, and a mesh size of 20 to 2000 meshes, preferably 50 to 500 meshes.
[0032] In a specific embodiment of the present invention, the concentrated acid is selected from one or more of sulfuric acid, nitric acid and perchloric acid, preferably sulfuric acid;
[0033] A0 is any concentration between M-10% and M+10%, preferably A0 is any concentration between M-5% and M+5%, A0 is the concentration of the concentrated acid, and M is the highest concentration of the analytical pure reagent grade of the concentrated acid.
[0034] In a specific embodiment of the present invention, the mass ratio of the concentrated acid to the graphite is (10-200):1, preferably (25-100):1.
[0035] In a specific embodiment of the present invention, the mass ratio of potassium permanganate to graphite is (1-10):1, preferably (3-8):1;
[0036] The mass ratio of potassium permanganate to graphite added in each batch is (0.1-2):1, preferably (0.2-1):1.
[0037] In a specific embodiment of the present invention, the method further comprises:
[0038] In step S1, after adding potassium permanganate, the temperature is controlled to below 40° C., preferably below 30° C., more preferably below 20° C., and stirred for 0.1 to 12 h, preferably 0.5 to 6 h; no nitrate is added during the reaction;
[0039] In step S2, the conditions of the heating reaction are: a temperature of 30 to 80°C, preferably 40 to 60°C, a reaction time of 0.2 to 12h, preferably 1 to 6h; the time for stirring with water is 0.1 to 6h, preferably 0.5 to 2h; the conditions of the spray drying include: an inlet temperature of 200 to 400°C, preferably 250 to 350°C, an outlet temperature of 120 to 300°C, preferably 150 to 200°C, and a feed rate of the mixed slurry of 10 to 10000ml / min, preferably 20 to 2000ml / min.
[0040] In a specific embodiment of the present invention, the water content of the mixed slurry is 50 to 95% by weight, preferably 70 to 90% by weight;
[0041] The mass ratio of the added amount of water to the added amount of the graphite is (10-500):1, preferably (20-250):1. In the present invention, the added amount of water is required to match the solid content of the mixed slurry entering the spray drying equipment with the steps and conditions of the spray drying.
[0042] The second aspect of the present invention provides a graphite oxide-based composite material prepared by the method provided by the first aspect of the present invention.
[0043] In a specific embodiment of the present invention, the graphite oxide-based composite material contains manganese, potassium, sulfur, carbon and oxygen. Based on the mass of the graphite oxide-based composite material, the manganese content is 20-50% by weight, the potassium content is 5-20% by weight, the sulfur content is 10-40% by weight, the carbon content is 5-30% by weight, and the balance is oxygen; preferably, the manganese content is 25-35% by weight, the potassium content is 8-15% by weight, the sulfur content is 15-30% by weight, the carbon content is 10-20% by weight, and the balance is oxygen.
[0044] The specific surface area of the graphite oxide-based composite material is 200 to 700 m 2 / g, preferably 400 to 600 m 2 / g, the pore volume is 0.5 to 2.0 ml / g, preferably 0.8 to 1.5 ml / g, and the average particle size is 0.5 mm or less, preferably 0.2 mm or less.
[0045] It should be noted that the graphite oxide-based composite material prepared by the present invention is a composition of graphite oxide, manganese oxide and manganese salt, etc. The graphite oxide-based composite material contains elements such as manganese, potassium, and sulfur, can react with sulfides, can effectively remove sulfides from materials, and exhibits excellent sulfide removal performance when used in reaction processes such as purification of sulfide-containing materials.
[0046] The third aspect of the present invention provides use of the graphite oxide-based composite material according to the second aspect of the present invention in removing sulfides.
[0047] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.
[0048] The reagents used in the present invention are all commercially available analytically pure reagents.
[0049] Example 1
[0050] a. Add 150 ml of concentrated sulfuric acid (mass concentration greater than 98%) and 5 g of graphite into a beaker to obtain a mixed solution;
[0051] b. Add 25 g of potassium permanganate into the mixed solution obtained in step a in 5 batches, and stir and mix at 10° C. for 1 h to obtain a mixed material;
[0052] c. Stir the mixture obtained in step b at 40°C under autogenous pressure for 2h;
[0053] d. Add 150 ml of water to the mixture in step c and continue stirring for 1 h to obtain a mixed slurry;
[0054] e The mixed slurry is sent into a spray dryer for drying, the inlet temperature is 300°C, the outlet temperature is 220°C, the feed rate of the mixed slurry is 50ml / min, and the graphite oxide-based composite material is obtained at the main outlet.
[0055] Example 2
[0056] The preparation method in Example 1 was adopted, except that, in step a, 100 ml of concentrated sulfuric acid was added.
[0057] Example 3
[0058] The preparation method in Example 1 was adopted, except that 15 g of potassium permanganate was added in step b.
[0059] Example 4
[0060] The preparation method in Example 1 was adopted, except that in step c, the reaction temperature was 30°C.
[0061] Example 5
[0062] The preparation method in Example 1 was adopted, except that in step d, 450 ml of water was added.
[0063] Example 6
[0064] The preparation method in Example 1 was adopted, except that in step b, the mass ratio of potassium permanganate to graphite added in each batch was 5:3, that is, potassium permanganate was added in 3 batches.
[0065] Example 7
[0066] The preparation method in Example 1 was adopted, except that in step e, the inlet temperature was 220°C and the outlet temperature was 120°C.
[0067] Example 8
[0068] The preparation method in Example 1 was adopted, except that in step a, 150 ml of concentrated nitric acid was added instead of concentrated sulfuric acid.
[0069] Comparative Example 1
[0070] The preparation method in Example 1 is adopted, except that in step b, 25 g of potassium permanganate is added once to the mixed solution obtained in step a.
[0071] Comparative Example 2
[0072] The preparation method in Example 1 was used, except that in step e, oven drying was used instead of spray drying, and the oven temperature was 220°C.
[0073] Test Case
[0074] The element content of the sample was determined by XPS on a VGESCA-LABS X-ray photoelectron spectrometer, using Mg Kα X-rays as the laser source and the C1s binding energy (284.6 eV) of the surface contamination carbon to calibrate the binding energy of each element in the desulfurizer surface species.
[0075] The warm nitrogen adsorption-desorption test (BET) was carried out on a JW-BK200C surface area and pore size analyzer produced by Beijing Jingwei Gaobo Co., Ltd. The specific surface area and pore volume were calculated using the two-parameter BET equation, and the pore distribution was calculated using the BJH method.
[0076] The sulfide content in the hydrogen before and after removal was analyzed by online chromatography (Nexis-2030, Shimadzu Corporation, Japan) and SCD fluorescence detector (SCD-2030).
[0077] 500 mg of the examples and comparative examples prepared by the present invention were loaded as catalysts into the constant temperature section of the reactor of a fixed bed micro reactor with an inner diameter of 10 mm and a length of 600 mm after passivation, and quartz sand was filled up and down. The hydrogen sulfide content in the hydrogen raw gas was 1000 ppm, and it was passed at a flow rate of 35 ml / min at 90°C and 2.0 MPa to remove the sulfide reaction. The hydrogen sulfide content in the hydrogen after the removal reaction was analyzed online, and the sulfide removal rate was calculated. The test results of the sulfide removal rate at 2h are shown in Table 1, and other characterization results of the prepared product are shown in Table 2.
[0078] Table 1
[0079] Sulfide removal rate / % Example 1 98 Example 2 92 Example 3 89 Example 4 90 Example 5 87 Example 6 93 Example 7 85 Example 8 71 Comparative Example 1 74 Comparative Example 2 58
[0080] Table 2
[0081]
[0082]
[0083] According to the test results in Table 1 and Table 2, it can be seen that the graphite oxide-based composite material prepared by the preparation method provided by the present invention has a larger specific surface area and pore volume than the comparative example, can react with sulfide, can effectively remove sulfide from the material, and exhibits excellent sulfide removal performance in the reaction process such as purification of sulfide-containing materials, and the removal rate of sulfide in the material reaches more than 90%; the preparation method of the present invention does not require the addition of nitrates, thereby reducing the cost of preparing materials, and the preparation process omits the step of terminating the reaction with a large amount of water, thereby reducing wastewater discharge.
[0084] It can be seen from the test results of Examples 1 to 8 that when the amount of potassium permanganate and the batch of addition, the drying method and drying conditions of the mixed slurry, the mass ratio of the amount of water added to the amount of graphite added, and the amount and type of concentrated acid are within the specified range of the present invention, the effect and performance of the product prepared by the present invention can be further improved.
[0085] It can be seen from the test results of Comparative Examples 1 to 2 that in Comparative Example 1, adding potassium permanganate to graphite at one time will cause uneven content of potassium permanganate adsorbed on graphite, resulting in a smaller specific surface area and pore volume of the prepared graphite oxide-based composite material, poor product performance, and a reduced removal rate of sulfides in the material; in Comparative Example 2, oven drying is used instead of spray drying, which will cause the specific surface area and pore volume of the prepared composite material to be significantly reduced, the product quality is reduced, and the sulfide removal rate is significantly lower than that in Example 1.
[0086] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0087] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0088] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a graphite oxide-based composite material, the method comprising: S1: adding graphite to concentrated acid and adding potassium permanganate in batches to obtain a mixed material; S2: After heating the mixed material for reaction, water is added and stirred to obtain a mixed slurry, and the mixed slurry is spray-dried to obtain a graphite oxide-based composite material.
2. The method according to claim 1, wherein: The graphite is one or more of natural flake graphite, natural cryptocrystalline graphite and artificial graphite; The graphite has a carbon content of more than 95% by weight, an ash content of less than 5%, and a mesh size of 20 to 2000 meshes.
3. The method according to claim 1, wherein: The concentrated acid is selected from one or more of sulfuric acid, nitric acid and perchloric acid; A0 is any concentration between M-10% and M+10%, preferably A0 is any concentration between M-5% and M+5%, A0 is the concentration of the concentrated acid, and M is the highest concentration of the analytical pure reagent grade of the concentrated acid.
4. The method according to claim 1, wherein: The mass ratio of the concentrated acid to the graphite is (10-200):1, preferably (25-100):
1.
5. The method according to claim 1, wherein: The mass ratio of the potassium permanganate to the graphite is (1-10):1, preferably (3-8):1; The mass ratio of potassium permanganate to the graphite added in each batch is (0.1-2):1, preferably (0.2-1):
1.
6. The method according to claim 1, wherein: The method further includes: In step S1, after adding potassium permanganate, the temperature is controlled to below 40° C., preferably below 30° C., more preferably below 20° C., and stirred for 0.1 to 12 hours; no nitrate is added during the reaction; In step S2, the conditions of the heating reaction are: temperature of 30-80°C, reaction time of 0.2-12h; the time of stirring with water is 0.1-6h; the conditions of the spray drying include: inlet temperature of 200-400°C, outlet temperature of 120-300°C, and feed rate of the mixed slurry of 10-10000ml / min, preferably 20-2000ml / min.
7. The method according to claim 1, wherein: The water content of the mixed slurry is 50 to 95% by weight, preferably 70 to 90% by weight; The mass ratio of the amount of water added to the amount of graphite added is (10-500):1, preferably (20-250):
1.
8. A graphite oxide-based composite material prepared by the method according to any one of claims 1 to 7.
9. The graphite oxide-based composite material according to claim 8, wherein: The graphite oxide-based composite material contains manganese, potassium, sulfur, carbon and oxygen. Based on the mass of the graphite oxide-based composite material, the manganese content is 20-50% by weight, the potassium content is 5-20% by weight, the sulfur content is 10-40% by weight, and the carbon content is 5-30% by weight; The specific surface area of the graphite oxide-based composite material is 200 to 700 m 2 / g, preferably 400 to 600 m 2 / g, the pore volume is 0.5 to 2.0 ml / g, preferably 0.8 to 1.5 ml / g, and the average particle size is 0.5 mm or less, preferably 0.2 mm or less.
10. Use of the graphite oxide-based composite material according to claim 8 or 9 in removing sulfides.