Method for processing colored LOGO on surface of aluminum alloy plate
Through laser coarseness and color coating paste printing technology, the color LOGO is formed on the surface of aluminum alloy, which solves the problem that the existing technology cannot achieve color LOGO and insufficient adhesion, and realizes the stable adhesion and durability of color LOGO on the surface of aluminum alloy.
Patent Information
- Application Number
- CN202411306130.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art cannot realize the processing of color LOGO on the surface of aluminum alloy, and the oxide film on the surface of aluminum alloy affects the adhesion of the coating material.
The wettability of the aluminum alloy surface is improved by laser roughening, and a colored LOGO is formed on the aluminum alloy surface using color coating slurry and steel screen printing technology, followed by sintering to improve adhesion.
The formation of colored LOGO on the surface of aluminum alloy is realized, and the adhesion of the coating material is improved. The process is simple and the cost is low. The obtained LOGO is stable, friction-resistant and acid-base-resistant.
Smart Images

Figure CN119056726A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy surface treatment, and specifically relates to a method for processing a colored LOGO on the surface of an aluminum alloy plate. Background Art
[0002] With the continuous development of aluminum alloy product processing industry, various aluminum alloy processing technologies are constantly improving, such as aluminum extrusion, aluminum stamping, aluminum milling, etc. As the market develops, the appearance and structure of similar products are becoming more and more consistent. In order to make the product stand out among similar appearance and structure products, new elements need to be added to the product appearance decoration.
[0003] At present, the technology of laser engraving on aluminum alloy surface is very mature, and it can realize engraving LOGO trademarks, text, QR code, pattern, serial number, running number, symbol on aluminum alloy shell, and it can realize engraving black, white, deep engraving, shallow engraving, and the engraved LOGO trademark has the advantages of never fading and never falling off. However, the method of directly laser engraving on the surface of aluminum alloy can only obtain black and white LOGO, and cannot realize color LOGO.
[0004] In addition, aluminum alloy is a relatively active metal, which easily reacts chemically with oxygen and moisture in the air to form compounds such as aluminum oxide, and forms a dense oxide film on the surface of the aluminum alloy. This oxide film is difficult to fully combine with the coating material, which affects the adhesion of the aluminum parts. However, after laser roughening the surface of the aluminum alloy, the wettability of the surface can be greatly improved, thereby improving the adhesion of the coating material. In summary, it is imperative to achieve a method of good adhesion of the color coating material on the surface of the aluminum alloy to form a color LOGO. Summary of the invention
[0005] The purpose of the present invention is to address the defects of the background technology. The present invention proposes a method for processing a colored LOGO on the surface of an aluminum alloy plate. The surface wettability of the aluminum alloy is improved by laser roughening, thereby improving the adhesion of the coating material, and enabling the colored coating material to adhere well to the aluminum alloy surface to form a colored LOGO.
[0006] The technical solution to achieve the purpose of the present invention is:
[0007] A method for processing a colored LOGO on the surface of an aluminum alloy plate comprises the following steps:
[0008] Step S1. Laser roughening, using a laser to physically roughen the surface of the aluminum alloy;
[0009] Step S2. properly cleaning the roughened aluminum alloy surface;
[0010] Step S3. preparing a color coating slurry by mixing pigment powder and glass powder to prepare a mixed powder, and adding an organic carrier to the mixed powder to prepare a color coating slurry;
[0011] Step S4. Steel plate printing, using a steel stencil to print the configured color coating slurry on the laser roughened area on the aluminum alloy surface;
[0012] Step S5. Drying the color pattern on the surface of the aluminum alloy;
[0013] Step S6. Sintering: using a box furnace to sinter the aluminum alloy printed with the colored glass enamel pattern to obtain a colored LOGO on the surface of the aluminum alloy. Preferably, in the step of laser roughening the surface of the aluminum alloy, the power of the laser used is 5W, the scanning speed is 1000mm / s, the frequency is 40kHz, the pulse width is 1μs, and the laser wavelength is 355nm.
[0014] Preferably, in the cleaning step S2, a slow water flow is required to rinse the surface of the aluminum alloy to remove metal powder particles generated during the laser physical roughening process to avoid affecting the subsequent color pattern printing.
[0015] Preferably, the configuration method of the color coating slurry in step S3 is as follows: commercial FD46 low-melting point glass powder and commercial high-melting point pigment powder are mixed in a ratio of 4:1, the mixed powder is mixed with an organic carrier in a ratio of 3:1, and stirred for 2 hours to obtain a uniform color coating slurry.
[0016] Preferably, the formula of the organic carrier in step S3 is 50wt% turpentine alcohol, 35wt% diethylene glycol butyl ether acetate, 5wt% dibutyl phthalate, 2wt% castor oil, and 8wt% ethyl cellulose.
[0017] Preferably, the configuration method of the organic carrier in step S3 is as follows: 50wt% turpentine alcohol, 35wt% diethylene glycol butyl ether acetate, 5wt% dibutyl phthalate, and 2wt% castor oil are added in sequence into a beaker, heated to 90°C under stirring conditions, 8wt% ethyl cellulose is added, and stirring is continued at 90°C for 60min until the ethyl cellulose is completely dissolved in the organic carrier.
[0018] Preferably, in step S4, the printing requires placing the laser-roughened aluminum alloy under the hollowed-out pattern of the steel mesh plate, and using a scraper to scrape the color coating slurry across the hollowed-out pattern to obtain a color pattern on the surface of the aluminum alloy.
[0019] Preferably, in step S5, the drying temperature is 60° C. and the drying time is 30 min.
[0020] Preferably, in step S6, the heating rate of the box furnace during sintering is set to 10°C / min, the temperature is raised to 350°C, and the temperature is kept at this temperature for 30 minutes to achieve the purpose of debinding and prevent the carbonization of the residual organic carrier from affecting the color development of the coating. The temperature is then continued to be raised to 450°C, and the temperature is kept at this temperature for 30 minutes before the furnace is cooled to room temperature.
[0021] Compared with the prior art, the present invention adopts the above technical solution and has the following beneficial effects:
[0022] 1. The present invention provides a method for processing a colored LOGO on the surface of an aluminum alloy plate, which uses a laser to roughen the surface of the aluminum alloy. It is a physical roughening method that does not require the use of highly corrosive chemicals, reduces harm to the environment and human body, and is a more green and environmentally friendly processing method.
[0023] 2. The present invention provides a method for processing a colored LOGO on the surface of an aluminum alloy plate. After the aluminum alloy surface is roughened by laser, the wettability of the surface is greatly improved, thereby improving the adhesion of the coating material.
[0024] 3. The present invention provides a method for processing a colored LOGO on the surface of an aluminum alloy plate, which uses a colored coating material to achieve the colorization of the LOGO on the surface of the aluminum alloy.
[0025] 4. The present invention provides a method for processing a colored LOGO on the surface of an aluminum alloy plate, which obtains a LOGO on the surface of the aluminum alloy by means of steel screen printing. Compared with other printing methods, the process operation is simple, convenient, fast and low-cost.
[0026] 5. The present invention provides a method for processing a colored LOGO on the surface of an aluminum alloy plate, in which a colored LOGO is sintered on a laser-roughened aluminum alloy surface. The obtained LOGO has firm adhesion, is resistant to friction, is resistant to acid and alkali, and has high reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a scanning electron microscope image of the original morphology of the aluminum alloy surface of the present invention;
[0028] Figure 2 This is a scanning electron microscope image of the aluminum alloy surface after laser roughening according to the present invention;
[0029] Figure 3 This is the optical image before sintering of the color LOGO printed on the surface of the aluminum alloy after laser roughening according to the present invention;
[0030] Figure 4 The optical image after sintering of the color LOGO printed on the surface of the aluminum alloy after laser roughening according to the present invention;
[0031] Figure 5The optical image before sintering of the color LOGO printed on the original aluminum alloy surface according to the present invention;
[0032] Figure 6 This is the optical image after sintering of the original aluminum alloy surface printed with a colored LOGO as described in the present invention. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The present invention discloses a method for processing a colored LOGO on the surface of an aluminum alloy plate, comprising the following steps:
[0035] Step S1. Laser roughening, using a laser to physically roughen the surface of the aluminum alloy;
[0036] Step S2. properly cleaning the roughened aluminum alloy surface;
[0037] Step S3. preparing a color coating slurry by mixing pigment powder and glass powder to prepare a mixed powder, and adding an organic carrier to the mixed powder to prepare a color coating slurry;
[0038] Step S4. Steel plate printing, using a steel stencil to print the configured color coating slurry on the laser roughened area on the aluminum alloy surface;
[0039] Step S5. Drying the color pattern on the surface of the aluminum alloy;
[0040] Step S6: sintering: using a box-type furnace to sinter the aluminum alloy printed with the colored glass glaze pattern to obtain a colored LOGO on the surface of the aluminum alloy.
[0041] In the step S1, laser roughening is to scan the surface of the aluminum alloy with a laser, the power of the laser used is 5W, the scanning speed is 1000mm / s, the frequency is 40kHz, the pulse width is 1μs, and the laser wavelength is 355nm.
[0042] In step S2, the cleaning requires using a slow water flow to rinse the aluminum alloy surface to remove the metal powder particles generated during the laser physical roughening process to avoid affecting the subsequent color LOGO printing.
[0043] In step S3, the color coating slurry is prepared as follows: commercial FD46 low melting point glass powder and commercial high melting point pigment powder are mixed in a ratio of 4:1, the mixed powder is mixed with an organic carrier in a ratio of 3:1, and stirred for 2 hours to obtain a uniform color coating slurry. The formula of the organic carrier is 50wt% turpentine alcohol, 35wt% diethylene glycol butyl ether acetate, 5wt% dibutyl phthalate, 2wt% castor oil, and 8wt% ethyl cellulose.
[0044] In step S3, the configuration method of the organic carrier is as follows: 50wt% of turpentine alcohol, 35wt% of diethylene glycol butyl ether acetate, 5wt% of dibutyl phthalate, and 2wt% of castor oil are added in sequence into a beaker, heated to 90°C under stirring conditions, 8wt% of ethyl cellulose is added, and stirring is continued at 90°C for 60 minutes until the ethyl cellulose is completely dissolved in the organic carrier.
[0045] In step S4, printing requires placing the laser-roughened aluminum alloy under the hollowed-out pattern of the steel mesh plate, and using a scraper to scrape the color coating slurry across the hollowed-out pattern to obtain a color LOGO on the surface of the aluminum alloy.
[0046] In step S5, the drying temperature is 70-80° C. and the drying time is 40-60 min.
[0047] In step S6, the heating rate of the box furnace during sintering is set to 10°C / min, the temperature is raised to 350°C, and the temperature is kept for 30 minutes to achieve the purpose of debinding and prevent the carbonization of the residual organic carrier from affecting the color development of the coating. The temperature is then continued to be raised to 450°C, and after keeping the temperature for 30 minutes, the furnace is cooled to room temperature.
[0048] Example 1
[0049] (1) Preparatory step: Prepare several 15×25 mm aluminum alloy plates and ultrasonically clean them in alcohol for 3 min.
[0050] (2) Laser roughening: Set the laser scanning area to 15×15 mm, the laser scanning speed to 1000 mm / s, the laser frequency to 40 kHz, the pulse width to 1 μs, and the wavelength to 355 nm. Turn on the laser red trace, place the aluminum alloy plate in the laser red trace area, ensure that the red trace area is in the center of the aluminum alloy plate, adjust the laser focal length, focus the laser on the upper surface of the aluminum alloy plate, and start laser scanning.
[0051] (3) Cleaning: Rinse the laser-roughened aluminum alloy with a slow water flow to remove the metal powder particles generated during the laser physical roughening process to avoid affecting the subsequent color LOGO printing.
[0052] (4) Preparation of organic carrier: 5 g of turpentine, 3.5 g of diethylene glycol butyl ether acetate, 0.5 g of dibutyl phthalate, and 0.2 g of castor oil were added to a beaker in sequence, and heated to 90°C under stirring. After adding 0.8 g of ethyl cellulose, stirring was continued at 90°C for 60 min until the ethyl cellulose was completely dissolved in the organic carrier.
[0053] (5) Color coating powder preparation: Add 8 g of commercial FD46 low-melting point glass powder, 2 g of commercial high-melting point pigment powder, and 20 ml of alcohol into a beaker, stir for 2 h to fully mix the commercial FD46 low-melting point glass powder and the commercial high-melting point pigment powder, pour into a watch glass, place in a 60°C constant temperature drying oven and dry for 2 h to obtain a uniform color coating powder.
[0054] (6) Color coating slurry preparation: Add 3 g of color coating powder and 1 g of organic carrier into a beaker in sequence and stir for 2 h to obtain a uniform color coating slurry.
[0055] (7) Stencil printing: Place the laser-roughened aluminum alloy under the hollow pattern of the stencil plate, and use a scraper to scrape the color coating slurry across the hollow pattern to obtain a color pattern on the aluminum alloy surface. Then, place the aluminum alloy with the color pattern in a constant temperature drying oven at 60°C and dry it for 30 minutes.
[0056] (8) Sintering: The aluminum alloy plate with the pattern printed on it that was dried in the previous step was placed in a box-type furnace. The heating rate was set to 10 °C / min. The temperature was raised to 350 °C and kept at this temperature for 30 min to achieve the purpose of debinding and prevent the carbonization of the residual organic carrier from affecting the color development of the coating. The temperature was then raised to 450 °C and kept at this temperature for 30 min. The furnace was cooled to room temperature to obtain aluminum alloy sample A with a colored LOGO on the surface.
[0057] like Figure 4 As shown, the colored LOGO on the sintered surface is reliably attached to the laser-roughened aluminum alloy surface and has uniform color development, which can meet the colorization requirements of the LOGO on the aluminum alloy surface.
[0058] Example 2
[0059] (1) Preparatory step: Prepare several 15×25 mm aluminum alloy plates and ultrasonically clean them in alcohol for 3 min.
[0060] (2) Preparation of organic carrier: 5 g of turpentine, 3.5 g of diethylene glycol butyl ether acetate, 0.5 g of dibutyl phthalate, and 0.2 g of castor oil were added to a beaker in sequence, and heated to 90°C under stirring. After adding 0.8 g of ethyl cellulose, stirring was continued at 90°C for 60 min until the ethyl cellulose was completely dissolved in the organic carrier.
[0061] (3) Color coating powder preparation: Add 9 g of commercial FD46 low-melting point glass powder, 1 g of commercial high-melting point pigment powder, and 20 ml of alcohol into a beaker, stir for 2 h to fully mix the commercial FD46 low-melting point glass powder and the commercial high-melting point pigment powder, pour into a watch glass, place in a constant temperature drying oven at 60-70°C and dry for 2 h to obtain a uniform color coating powder.
[0062] (4) Color coating slurry preparation: Add 3 g of color coating powder and 1 g of organic carrier into a beaker in sequence and stir for 2 h to obtain a uniform color coating slurry.
[0063] (5) Stencil printing: Place the aluminum alloy under the hollow pattern of the stencil plate, and use a scraper to scrape the color coating slurry across the hollow pattern to obtain a color pattern on the aluminum alloy surface. Then, place the aluminum alloy with the color pattern in a constant temperature drying oven at 70-80°C and dry it for 40-60 minutes.
[0064] (6) Sintering: The aluminum alloy plate with the pattern printed on it that was dried in the previous step was placed in a box-type furnace, and the heating rate was set to 10°C / min. The temperature was raised to 350°C and kept at this temperature for 30 minutes to achieve the purpose of debinding and prevent the carbonization of the residual organic carrier from affecting the color development of the coating. The temperature was then raised to 450°C and kept at this temperature for 30 minutes. The furnace was then cooled to room temperature to obtain aluminum alloy sample B with a colored LOGO on the surface.
[0065] like Figure 6 As shown in the figure, the colored LOGO on the surface fell off after sintering and failed to achieve reliable adhesion to the aluminum alloy surface.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for processing a colored LOGO on the surface of an aluminum alloy plate, characterized in that: The method comprises the following steps: Step S1. Laser roughening, using a laser to physically roughen the surface of the aluminum alloy; Step S2. properly cleaning the roughened aluminum alloy surface; Step S3. preparing a color coating slurry by mixing pigment powder and glass powder to prepare a mixed powder, and adding an organic carrier to the mixed powder to prepare a color coating slurry; Step S4. Steel plate printing, using a steel stencil to print the configured color coating slurry on the laser roughened area on the aluminum alloy surface; Step S5. Drying the color pattern on the surface of the aluminum alloy; Step S6: sintering: using a box-type furnace to sinter the aluminum alloy printed with the colored glass glaze pattern to obtain a colored LOGO on the surface of the aluminum alloy.
2. The method for processing a colored LOGO on the surface of an aluminum alloy plate according to claim 1, characterized in that: In laser roughening, the process of physically roughening the ceramic surface: the laser type is ultraviolet laser, the power is 5W, the scanning speed is 1000mm / s, the frequency is 40kHz, the pulse width is 1μs, and the wavelength is 355nm.
3. The method for processing a colored LOGO on the surface of an aluminum alloy plate according to claim 1, characterized in that: After the aluminum alloy plate is laser roughened, the aluminum alloy surface is rinsed with a slow stream of water to remove particles generated during the laser physical roughening process to avoid affecting the subsequent color pattern printing.
4. The method for processing a colored LOGO on the surface of an aluminum alloy plate according to claim 1, characterized in that: The formula of the organic carrier is 50wt% turpentine alcohol, 35wt% diethylene glycol butyl ether acetate, 5wt% dibutyl phthalate, 2wt% castor oil, and 8wt% ethyl cellulose.
5. The method for processing a colored LOGO on the surface of an aluminum alloy plate according to claim 1, characterized in that: The organic carrier is prepared as follows: 50 wt% turpentine alcohol, 35 wt% diethylene glycol butyl ether acetate, 5 wt% dibutyl phthalate, and 2 wt% castor oil are sequentially added into a beaker, heated to 90° C. under stirring conditions, 8 wt% ethyl cellulose is added, and stirring is continued at 90° C. for 60 min until the ethyl cellulose is completely dissolved in the organic carrier.
6. The method for processing a colored LOGO on the surface of an aluminum alloy plate according to claim 1, characterized in that: The color coating slurry is prepared as follows: commercial FD46 low-melting-point glass powder and commercial high-melting-point pigment powder are mixed in a ratio of 4:1, the mixed powder is mixed with an organic carrier in a ratio of 3:1, and stirred for 2 hours to obtain a uniform color coating slurry.
7. The method for processing a colored LOGO on the surface of an aluminum alloy plate according to claim 1, characterized in that: The dried colored LOGO was sintered with a heating rate of 10°C / min to 350°C and kept warm for 30 minutes to achieve the purpose of debinding and prevent the carbonization of the residual organic carrier from affecting the color of the coating. The temperature was then continued to rise to 450°C and kept warm for 30 minutes before the furnace was cooled to room temperature.
Citation Information
Patent Citations
Sintered lead-free low-temperature silver paste thick film method for surface modification of aluminum alloy
CN109797392A
Method for preparing fine ceramic circuit board through laser-assisted chemical plating
CN117966136A
Al2O3 ceramic tube shell, conductive nickel slurry thereof and preparation method of Al2O3 ceramic tube shell
CN118039218A
Improvements in method of decorating metal surfaces
GB191771A
Improvements in or relating to printing elements
GB866070A